It depends what type of defects you want to check.
Like porosity - you can use a wet electrode or long arc
Cracks - Embed Copper wires on carbon steel plates and weld
Lack of Fusion - Ask your welder to not to fuse the side wall of the Joint
Thanks & Regards
J.Gerald Jayakumar
00968-93281596
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
00968-93281596
From: Ali Asghari <asghariali@rocketmail.com>
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Sent: Tuesday, August 28, 2012 8:46 AM
Subject: [MW:15141] artificial defect
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Sent: Tuesday, August 28, 2012 8:46 AM
Subject: [MW:15141] artificial defect
Dear All
We want to demonstrate a phased array procedure with welded samples that have defects.
Does anybody know procedure/informations about making a weld with defects for qualification of NDT procedure?
Regards.
We want to demonstrate a phased array procedure with welded samples that have defects.
Does anybody know procedure/informations about making a weld with defects for qualification of NDT procedure?
Regards.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Comments