Mr. Mohemmed,

Any E 7018 electrode including H4R type gives minimum impact values up to -30 deg C only.
You should have gone for E 7018-1, E 7018 G (or) E 7018 H4R -spl. type electrodes
which has some extra Manganese and gives min. impact of 27 joules at - 46 deg C.

Hence pl. check and test the present lot . If the results are different, you have no option but to
go as per clients requirement.

sridhar.
 


From: Raghuram Bathula <raghurambathula@gmail.com>
To: Materials & Welding <materials-welding@googlegroups.com>
Sent: Wednesday, 22 August 2012 4:34 PM
Subject: [MW:15106] Re: electrode with diff impact temp mixing during welding.

test those electrodes for impact at -46 °C and convince your client.

On Aug 22, 11:16 am, mohd <mohd52...@gmail.com> wrote:
> dear experts,
>
> We have land in difficult situtuation due to welders mistakes.
>
> Electrode E7018H4R impact require -46deg but by mistakes welder used
> some electrodes E7018H4R -29deg during welding of 3 long seam 25m
> (filling n caping)
>
> Materials      516 gr 60    thk 40t.
> Process        GTAW+SMAW
>
>  What could be solution? To save joint.
> Client already given cut out.
>
> Regards,
> Mohammed.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.




No comments:

[MW:35633] IP Joint

Hello experts, I would like to know what is IP joints in piping(31.3)?  Regards Saurabh -- https://materials-welding.blogspot.com/...