Re: [MW:15112] Material as per SA 516 Gr.70 n

SA-516 Gr.70N is normalised state of SA-516 Gr.70. Per the ASME SA-516 Specification, plates under 1.5" in thickness can be supplied in the hot rolled or hot worked condition. For plates 1.5" and over, the plates must be supplied in the normalized condition unless specified by the Purchaser. 
 
If your application requires notch toughness testing, the plates need to be re-heat treated after forming to be in the normalized condition per the Specification unless you specify otherwise. Plates that are hot worked and air cooled after hot working are not considered to be normalized. This is a separate heat treatment step.
Hope this help.


From: Amit Udavant <amitudavant@gmail.com>
To: materials-welding@googlegroups.com
Sent: Wednesday, August 22, 2012 8:54 AM
Subject: [MW:15104] Material as per SA 516 Gr.70 n


Dear all
Please tell me more about CS Plates as per SA 516 Gr.70 N. Is it different from  SA 516 Gr.70? Or even a NormalisedSA 516 Gr.70 plate is equivalent  to SA 516 Gr.70 N? Please also let me know how to recognise the authenticity fronm the material TCs.
--
Warm Regards
amit
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 


No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...