Re: [MW:15116] Ferrite Number

In schaeffler diagram, Ni equivalent is calculated on Ni, C, Mn &  Cr equivalent is based up on Cr, Mo, Si, Cb. Delong  diagram in addition to above takes note of nitrogen, a strong astenitiser.

Delta Ferrite: Depending on the relative proportions of ferrite and austenite forming elements present, the  weld metal solidifies initially as grains of delta ferrite or grains  of asutenite. As solidification proceeds, initial ferrite grains transform to austenite grains. If ferrite forming elements are more, delta ferrite forms in the micro structure. If the structure is austenite, it remains austenite till the end of solidification.

Ferrite % & Ferrite no: Schaeuffler used metallographic method for determining the ferrite percentage (%) in the weld metal, Delong has used a magnetic measuring instrument (Magne Gauge)  in his work. Delong has adopted an arbitrary standard called Ferrite Number (FN) to indicate the ferrite content. Metallographic measurements are helpful but difficult to run accurately due to small size of ferrite particles.

Ferrite % and Ferrite Number are identical at low levels of ferrite, but they differ widely when Ferrite levels are high.

Variation of Ferrite in your measurement:  Ferrite content as claimed by the manufacturer in his batch report can be reproduced on production welds,  only when correct welding procedure is used i.e., with controlled heat in put, use of smaller size electrodes, stringer bead runs, faster cooling rates, low inter pass temperature etc.   Use of high currents will also increase the ferrite level and  reduce the resistance to corrosion.

At times use of long arc and in-adequate shielding may induce Nitrogen (a strong austenitiser) into the weld and may reduce the ferrite levels to some extent.


Trust above details will help you to overcome your problems.

sridhar.
---------------------------------------------------------------------------------------------------


From: meisam shokri arfaei <meisamshokri@gmail.com>
To: materials-welding@googlegroups.com
Sent: Wednesday, 22 August 2012 4:25 PM
Subject: Re: [MW:15105] Ferrite Number

As I know 100FN is approximately shows 65% of ferrite volume, so this is the reason for the difference between FN and ferrite VOL%.
As you can see in below diagram the relation between FN and ferrite VOL% have been shown.
Also when you follow the standard procedure for evaluating FN the deviation of ±2 (approximately) is not prevented. So assume the deviation when you didn't follow standard procedure.

 



--
M. Shokri Arfaei
International Welding Engineer (IWE)
ASNT NDT Level III
ERI Metallurgy Lab. Manager
Tel: +98-21-66282127
Fax: +98-21-66282779
 
Please don't print this e-mail unless you really need to. BeGreen!

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 


Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...