[MW:13559] REGARDING PWHT of STORAGE TANK CLEAN OUT DOOR.

Manoj,

 

This PQR is acceptable, it is qualified for the design thickness as mentioned below. PQR with higher soaking time is qualified for lower soaking time also as per  QW- 407.2.

 

Note any change of PWHT (T&T) is a supplementary essential variable (i.e. where  notch-toughness requirement applies ), which is not the case here.

 

Thanks.

 

Pradip Goswami,P.Eng.IWE

Welding & Metallurgical Specialist & Consultant

Ontario, Canada.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

size=2 width="100%" align=center tabindex=-1>

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of manoj john
Sent: Monday, January 23, 2012 10:26 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:13554] REGARDING PWHT of STORAGE TANK CLEAN OUT DOOR.

 

Applicable Code is  ASME SEC IX.

Impact test not required.

On Mon, Jan 23, 2012 at 12:49 PM, james gerald <gerry_tup@yahoo.com> wrote:

Please give the detail of the applicable code and whether Impact test is required based on MDMT

 

Thanks & Regards J.Gerald Jayakumar 0091-9344954677


Sent: Saturday, January 21, 2012 7:55 PM


Subject: [MW:13536] REGARDING PWHT of STORAGE TANK CLEAN OUT DOOR.

 

Dear All,

 

I intended to use the following  WPS  for  storage tank clean out door welding :

 

Test coupon thickness  -   40 mm.

Material                       -   SA 516 Gr 70

Welding process          -   SMAW.

Electrode                    -    E 7018-1

PWHT  Temperature     -   620 - 650 degree centigrade.

Soaking time               -   180 minutes.

Rate of heating            -   130 Degree centigrade.

Rate of heating            -   130 Degree centigrade.

 

Storage tank detail:

Shell thickness              - 18 mm

Annular plate thickness  -  20 mm

Clean out door neck       -  18 mm

Clean out door flange      -  20 mm

Material                         -  SA 516 Gr 70

Welding process            -   SMAW

Electrode                       -   E 7018 -1

Stress relieving temp      -   620 - 650 degree centigrade.  

Soaking time                 -   60 minutes.

Rate of heating              -   150 - 200 Degree centigrade.

Rate of heating              -   150 - 200 Degree centigrade

 

My doubt is whether the soaking time in the PQR is acceptable or I have to qualify another WPS.

 

Thanks in advance.

Manoj

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...