The problem may be at the dilution between your filler metal and the P5 material. So based on the skills of the welder you can assume a dilution and calculate the FN with the WRC diagram
Best regards
Dr Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
HBS Regional Technical Manager
From: james gerald [gerry_tup@yahoo.com]
Sent: 06/12/2011 03:01 PST
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Subject: Re: [MW:13152] Dissimilar welding SS 316 to A335GrP5
Dr.George,
How do check Ferrite number in Inconel welds. Is it by Magnetic method.
I suppose this could be done only by calculating the Dilution.
Does Ferrite number prevents Hot cracking in Inconel welds. What is the significance.
Thanks & Reagrds
J.Gerald Jayakumar
00968-93281596
J.Gerald Jayakumar
00968-93281596
From: "george.dilintas@gr.bureauveritas.com" <george.dilintas@gr.bureauveritas.com>
To: materials-welding <materials-welding@googlegroups.com>
Sent: Tuesday, December 6, 2011 2:34 PM
Subject: Re: [MW:13151] Dissimilar welding SS 316 to A335GrP5
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
To: materials-welding <materials-welding@googlegroups.com>
Sent: Tuesday, December 6, 2011 2:34 PM
Subject: Re: [MW:13151] Dissimilar welding SS 316 to A335GrP5
Provided you do not get a FN lower than 5
Best regards
Dr Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
HBS Regional Technical Manager
Best regards
Dr Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
HBS Regional Technical Manager
From: james gerald [gerry_tup@yahoo.com]
Sent: 06/12/2011 01:42 PST
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Subject: Re: [MW:13150] Dissimilar welding SS 316 to A335GrP5
Sent: 06/12/2011 01:42 PST
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Subject: Re: [MW:13150] Dissimilar welding SS 316 to A335GrP5
It would be better to butter the P5 portion say 5 mm with ENiCrMo3, perform PWHT and weld it with 316SS .
Thanks & Reagrds
J.Gerald Jayakumar
00968-93281596
J.Gerald Jayakumar
00968-93281596
From: "george.dilintas@gr.bureauveritas.com" <george.dilintas@gr.bureauveritas.com>
To: materials-welding <materials-welding@googlegroups.com>
Sent: Tuesday, December 6, 2011 12:46 PM
Subject: Re: [MW:13149] Dissimilar welding SS 316 to A335GrP5
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
To: materials-welding <materials-welding@googlegroups.com>
Sent: Tuesday, December 6, 2011 12:46 PM
Subject: Re: [MW:13149] Dissimilar welding SS 316 to A335GrP5
I would not suggest to direct them directly. What are your thicknesses?
Best regards
Dr Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
HBS Regional Technical Manager
Best regards
Dr Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
HBS Regional Technical Manager
From: "Ashok Raman B Kutty \(MNT/PPTSB\)" [ashokraman_kutty@petronas.com.my]
Sent: 06/12/2011 09:27 ZE8
To: <materials-welding@googlegroups.com>
Subject: [MW:13145] Dissimilar welding SS 316 to A335GrP5
Sent: 06/12/2011 09:27 ZE8
To: <materials-welding@googlegroups.com>
Subject: [MW:13145] Dissimilar welding SS 316 to A335GrP5
We need to weld a SS 316 Return bend to 5 Chrome, 0.5 Mo alloy steel furnace tube. The electrode proposed is ENiCrMo3. The return bends are in a header box adjacent to the radiant section (horizontal tube furnace – crude distillation unit).
Is PWHT required to be done after welding?
Thanks
Ashok
DISCLAIMER : This e-mail and any files transmitted with it ("Message") is intended only for the use of the recipient(s) named above and may contain confidential information. You are hereby notified that the taking of any action in reliance upon, or any review, retransmission, dissemination, distribution, printing or copying of this Message or any part thereof by anyone other than the intended recipient(s) is strictly prohibited. If you have received this Message in error, you should delete this Message immediately and advise the sender by return e-mail. Opinions, conclusions and other information in this Message that do not relate to the official business of PETRONAS or its Group of Companies shall be understood as neither given nor endorsed by PETRONAS or any of the companies within the Group.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
No comments: