[MW:4115] FW: 4105] Pitting acceptance criteria

 

Mr Kader,

 

A-860 fittings have to conform to  requirements of  A/SA-960 specification (Spec for Common requirements for Wrought Fittings). As per A/SA-960 clause 15.3.2 fittings may be  ground  to sound metal ,repaired and blended to  the smooth. Some specific restrictions apply for fittings corresponding to MSS-SP-75.

 

In course of grinding, if the wall thickness is reduced below the nominal wall thickness , fittings may be rejected or repaired. However if the fittings are intended for sour-gas transmission or any other hydrocarbons, the repair has to be very selective and controlled.

 

If there is no choice but to use the damaged fittings, you may perform a Fitness for Service Evaluation, as per API-579 (Chapter-6). A Level-1, or 2 assessment may predict the safe service life of the components.

 

Thanks.  

 

Pradip Goswami,P.Eng , IWE 

Senior Engineer/Specialist(Welding-Metallurgy)

Engineering & Training Services Division

ONTARIO POWER GENERATION Inc.

PO Box-2000, RR-55(South)

Nanticoke, Ontario,N0A1L0

Tel:-(519) 587-2201, Ext 3107--in Nanticoke

         (416) 231-4111, Ext 5925--in Kipling,Toronto

Fax: (519) 587-6814

Email-pradip.goswami@opg.com.

 

From: pgoswami [mailto:pgoswami@quickclic.net]
Sent: Saturday, February 20, 2010 6:28 AM
To: GOSWAMI Pradip -THERMAL
Subject: FW: 4105] Pitting acceptance criteria

 

 

 

Pradip Goswami

88,Garth Trails Crescent

Hamilton, Ontario, L9B2X1,Canada

Email-pgoswami@sympatico.ca

Email-pgoswami@quickclic.net

Tel-905-679-9677

 

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Gulam kader
Sent: Wednesday, January 20, 2010 4:52 AM
To: materials-welding@googlegroups.com
Subject: [MW:4105] Pitting acceptance criteria

Dear all,

 

We received one 40" elbow (ASME 16.9) ASTM A 860 material having so much pitting on full external surface. Which standard we can refer for the acceptance criteria? 

 

 

I referred in ASTM A 860, its talks about only depth of surface discontinuity(5% of the nominal thickness),  there is no detail about the area of the pitting allowance.

 

Please help me on this issue. Very urgent

 

Regards,

 

Gulam Kader 


THIS MESSAGE IS ONLY INTENDED FOR THE USE OF THE INTENDED RECIPIENT(S) AND MAY CONTAIN INFORMATION THAT IS PRIVILEGED, PROPRIETARY AND/OR CONFIDENTIAL. If you are not the intended recipient, you are hereby notified that any review, retransmission, dissemination, distribution, copying, conversion to hard copy or other use of this communication is strictly prohibited. If you are not the intended recipient and have received this message in error, please notify me by return e-mail and delete this message from your system. Ontario Power Generation Inc.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...