[MW:3560] Re: PT after root pass in SS welding

Dear Mr.Devang Naik

What is meant by hot MT ?
Is it possible for Austenitic Stainless Steels ?

Regards

Prem Nautiyal
Godrej,Mumbai
Cell:9820313278

On Tue, 27 Oct 2009 20:49:24 +0530 wrote
>Dear Mr. Syed and Mr. Prem
>

>
You may go for hot MT after root pass.
>

>
Thanks
>

>
Devang Naik
>

>
On Tue, 27 Oct 2009 11:22:17 +0530 wrote
>
>
>
>
>
Hello Syed
>
>
>

>
>
>
You can very well conduct PT after Root pass while welding SS, only ensure that temp. has come below 52 degreeC.
>
>
>
We regularly conduct PT after root pass when welding SS jobs even upto 70mm thick with GTAW.
>
>
>

>
>
>
The chances of cracking after GTAW root pass is seen in thick sections of CS and LAS material i.e above 20/25mm thick OR having high restraints. Hence while welding such materials,we conduct PT after hot pass only.
>
>
>
For thin sections LPT can be done safely after root pass for CS/LAS material.
>
>
>
This is only my experience which i would like to share with you!!
>
>
>

>
>
>
Regards
>
>
>

>
>
>
Prem Nautiyal
>
>
>
Godrej, Mumbai
>
>
>
Cell:9820313278
>
>
>

>
>
>
On Sun, 25 Oct 2009 17:12:07 +0530 wrote
>
>
>
>Recently I faced the following issue and kindly clarify my doubt. A qualified WPS for stainless steel (A312-TP304H) requires PT after root pass. After root pass, its not possible to perform PT immediately unless the temperature reduces.
>
>
>
But, in normal practice,any weld is not to be stopped before completing hot pass or 1/3rd of groove thickness. I got difficulty in following both conditions on single weld joint.
>
>
>
Based on the above different opinions, kindly suggest me the right one with details.
>
>
>

>
>
>
PREM S NAUTIYAL
>
>
>
CELL : 9820313278


PREM S NAUTIYAL
CELL : 9820313278
--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...

Pages

Contributors

Blog Archive