Hi

We had successfully welded and qualified a procedure to weld ASTM A473 Type 431,UNS:S43100 forging.
We had welded with SMAW:E309L.
Preheat and interpass was 250 degree C.
After completion of welding wrap in glass wool/asbestos for slow cooling.

No PWHT required.

Regards

Prem Nautiyal
Cell:9820313278

On Thu, 08 Oct 2009 17:21:16 +0530 wrote
>if you are referring to 431(UNS S43100) stainless, can be welded with AWS E/ER410.To avoid cracking, pre-heat the workpiece to 400-600 F (204-316 C). After air cooling, treat at 1200 F (649 C) to reattain maximum properties.

On Thu, Oct 8, 2009 at 3:43 PM, Narendra Gohil wrote:
Dear All, Please help me to find out exact consumable to weld A 431.(1.4044) material for any process whether GTAW  or  SMAW.
Cr-15-18%,Ni-2/3%,Mn-1%. Thanks & Regards----------------------------Narendra GohilWelding EngineerQAFCOPh.00974-4228289(O)
Mo.00974-6044289Email: ngohil@qafco.com.qaP Save a tree.  Please don't print this e-mail unless it's really necessary.

PREM S NAUTIYAL
CELL : 9820313278
--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...

Pages

Contributors

Blog Archive