Saturday, March 29, 2008

[MW:701] Re: 698] Re: PMI TESTING OF SS 304L

XRF can only detect elements with atomic numbers greater than 21 i.e.
starting with Titanium onwards. Therefore, it cannot quantify C, S, P, etc.
So, it can tell the difference between SS304 and SS316, but not SS316 and
SS316L.

OES can detect all the elements including carbon, so it can be used very
conveniently for segregating even SS316 and SS316L.

Regards,

Kartik Iyer.
ELCA Laboratories.


----- Original Message -----
From: "Bathula Raghuram (Mumbai - PIPING)" <R.Bathula@ticb.com>
To: <materials-welding@googlegroups.com>
Sent: Thursday, March 27, 2008 7:22 PM
Subject: [MW:699] RE: 698] Re: PMI TESTING OF SS 304L


that's one of the main diff between OES and XRF analysers, where XRF
analysers can't detect %C and trace elements like S,P etc....


-----Original Message-----
From: materials-welding@googlegroups.com on behalf of shailesh dave
Sent: Wed 26/03/2008 18:30
To: materials-welding@googlegroups.com
Subject: [MW:698] Re: PMI TESTING OF SS 304L

DEAR PINAKIN,

THANKS FOR THE REPLY. IN THAT CASE HOW TO DIFFERNTIATE SS304 FROM 304L AND
SS316 FROM 316L. IF WE CAN NOT ANALYSE CARBON %.

REGARDS,

S.N.DAVE

pinakin jani <pbjani50@yahoo.co.in> wrote:
Dear Dave,
PMI can tell you the % of the contains like Ni, mo etc. Based on this % we
can check our requirement.

Regards,

Jani Pinakin


----- Original Message ----
From: Bathula Raghuram (Mumbai - PIPING) <R.Bathula@ticb.com>
To: materials-welding@googlegroups.com
Sent: Monday, 24 March, 2008 2:42:02 PM
Subject: [MW:686] PMI TESTING OF SS 304L

Probably spectro isort by Amtek can detect C, (thou I have not
used it), you can try at www.spectro.com

Also Arcmet930 by Metorex can detect C


---------------------------------

From: shailesh dave [mailto: snd2988@yahoo.com ]
Sent: Monday, March 24, 2008 2:07 PM
To: materials-welding@googlegroups.com
Subject: PMI TESTING OF SS 304L


DEAR MEMBERS,

CAN ANYBODY TELL ME WHAT TECHNIQUE SHOULD BE USE TO PERFORM PMI OF
SS304L. SINCE CARBON ANALYSIS IS VERY VERY IMPORTANT.

REGARDS,

S.N.DAVE

QA/QC MANAGER - TATA PROJECTS,

IWPP -III, SHUIBAH , SAUDI ARABIA


---------------------------------
Get the freedom to save as many mails as you wish. Click here to know how.


---------------------------------
Be a better friend, newshound, and know-it-all with Yahoo! Mobile. Try it
now.


--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...