Re: [MW:3954] PWHT

As per B31.3,2006 edition for carbon steel greater than 20mm PWHT required.Not 19mm as mentioned in Mr Ramprasad chari mail. 

On Mon, Jan 4, 2010 at 9:45 AM, Jimmy Nielsen <nielsen.jimmy@gmail.com> wrote:
Please look into table 331.1.1Requirements for Heat treatment:

According to different P or S number PHWT requirements are N/A, <13mm,
<19mm or ALL

Find you P or S number and look into the table and will have the answer,

Regards, jimmy



2010/1/4 Ramprasad Chari <ramprasad.chari@gmail.com>:
> PWHT for fabrication as per B31.3 calls for thk 3/4" and above
> Regards
> Aarpee
>
> On Sun, Jan 3, 2010 at 5:53 PM, Material-Testing 001 <murtuza1982@gmail.com>
> wrote:
>>
>> Please advise teh PWHT teratment requirmnet for seamless and welded
>> carbon steel pipes to A53 Grade B as per B31.3
>>
>> can you please let me know under what condition PWHT is mandatory?
>>
>> appreciate you feedbacks.
>>
>> --
>> To post to this group, send email to materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding-unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>> The views expressed/exchnaged in this group are members personel views and
>> meant for educational purposes only, Users must take their own decisions
>> w.r.t. applicable code/standard/contract documents.
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding-unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
With Warm regards,

G.Padmanabhan
+96895685853

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34919] Welder qualification certificate

Dear All     anyone can share a format for welder certificate and card format        Thanks & Best Regards Saleem manhappulath Mob:+9665...