Skip to main content

Re: [MW:33970] Weldability of A283 Gr C with A573 Gr70

There are certain factors to be considered while selecting the welding consumable.

1. The Tensile strength of the welding consumable shall be higher than the minimum specified Tensile strength of the Base material.
2. If two different grades are welded the welding consumable tensile strength shall be higher than the lowest grade.
Inline image

3. If it is a structural weld and welding to the pressure boundary then low H2 electrode is preferred such as E7018 / E7108-1.

4. If it is between a non pressure part to non-pressure part then  you can prefer E6013 for your requirement and thickness.
Inline image
5. If the Thickness(>25mm) & Carbon equivalent is higher it is preferred to weld with a low H2 electrode such as E7018

Thanks & Regards

J.Gerald Jayakumar




On Friday, 27 January, 2023 at 11:05:33 am GMT+3, Benaouda Mezrar <mezrarbenaouda4@gmail.com> wrote:


A573 gr 70 12mm 
A283 gr C 10mm

On Fri, 27 Jan 2023, 05:21 'james gerald' via Materials & Welding, <materials-welding@googlegroups.com> wrote:
Also provide the thickness 


On Thu, 26 Jan 2023 at 12:23, james gerald
What is the design CODE API 620 / 650


On Thu, 26 Jan 2023 at 12:19, Benaouda Mezrar
But sir we use these two nuances for construction of storage tanks. Is it applicable ? with different thickness 
sir please could you give me more arguments about the weldability of these two nuances ? 
thank you a lot for your helps sir    

Le jeu. 26 janv. 2023 à 07:40, 'james gerald' via Materials & Welding <materials-welding@googlegroups.com> a écrit :
Use E7018 / E7018-1


On Thu, 26 Jan 2023 at 7:32, Benaouda Mezrar
Dear friend 

could anyone answer my question, the question is : could we weld A573 GR70 with A283GR C
In my opinion we can't  weld them because the minimum specified  tensile are 
for A283 GR C = 380 MPA
for A573 Gr70 = 485 MPA

Please friend help me i need this information emergency

if the answer is yes which type of filler metal we should use for SMAW 




 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/20e0e61e-9ee4-4ef3-9080-fe83ae9c39ban%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/2043007948.1323331.1674715164817%40mail.yahoo.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANKYR7tUR_QCCPS-j8BRPq7tPAhjZqh2fD-kYKc72h%2BB_2Z0RQ%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1487907621.1327855.1674725111818%40mail.yahoo.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANKYR7tJdhQOR4aud6MWGqznhh7E7UTYQi0jwC%3DK54yBjOk2vg%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Re: [MW:14950] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

Dear All, I have been a CONSULTANT FOR such problem & my personal opinion is expressed as follow. I fully agree with views expressed so far. But bag to differ that " Code is a law, with engineering judgments. Hence the inspector has the rights to declare that the original HT was inadequate." Inspectors & total industry must resist the "REJECTION" . We as intellectual & having seniority must become practical. How the code will revise???. ANS.: One is experiments (Pure research) & second is such chances that gives opportunity to experiment !!! _______________________________________________________________________________________________ My understanding is that it is P1 material. In that case every pass normalizes the immediate bottom pass. Hence code requirement for P1 FOR MANDATORY SR is 32 mm & above thickness. SOLUTION:  In any case 0. After SR=PWHT no PTC testing is required as per code--Unless for low temp. vessels. That means code ...