Skip to main content

RE: [MW:32830] Re: REQUIRED FILLER WIRE FOR (ASTM A312-Gr UNS 31254) Super Austenitic Stainless Steel

Hello,

 

Alloy 625 (as highlighted below)  is the default electrode/ filler metal recommended for welding of ASTM A312-Gr UNS 31254 , 6Mo stainless steels. Download this Metrode publication from the link as mentioned below. You'll get a comprehensive guideline for welding of this alloy.

 

Welding of this alloy not very easy, it's tricky as like DSS/SDSS. You need to have good welding control.

 

How this would be of help.

 

Thanks.

 

Pradip Goswami.P.Eng, IWE.

Independent Welding & Metallurgical Engineering Specialist

Consultant: SNC Lavalin Inc. (Nuclear &Non-Nuclear)

Saudi Aramco Approved Designated Project Welding Engineer (DPWR)

Qatar Petroleum Approved, SME-Materials & Corrosion Engineering.

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@rogers.com,pradip.goswami@gmail.com

Cell/Whasapp:1-905-9793232

 

[PDF] FILLER MATERIALS FOR 6%Mo SUPERAUSTENITIC STAINLESS STEELS - Free Download PDF (silo.tips)

From: Muhammad Azeem <azeem7999@gmail.com>
Sent: February 8, 2022 11:23 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:32826] Re: REQUIRED FILLER WIRE FOR (ASTM A312-Gr UNS 31254) Super Austenetic Stainless Steel

 

Dear Siraj,

Thanks for your valuable response, Avesta P54 is a Brand ,I need to check if this manufacturer is approved by Aramco SAP & What is the AWS/SFA number for this filler wire ??

 

As I consult with 3rd Party they recommend  ERNiCrMo3,F43  ??

 

Regards,

Muhammad Azeem Iqbal

Welding Inspector Aramco Approved

053110-8577/0554453626/0590071467

 

 

On Wed, 9 Feb 2022 at 06:18, Mohd Siraj <mohd52100@gmail.com> wrote:

Avesta P54 is a good choice for SAS and it is affluently available in KSA, very cost effective.

just take care of good cleaning and avoid any kind of moisture on the surface and hope u pass G48!

On Tuesday, February 8, 2022 at 6:18:00 AM UTC+3 Muhammad Azeem wrote:

Gents,

I need your valuable support to assist about the filler wire to be used for Super Austenitic Stainless Steel (ASTM A 312 Gr UNS 31254) ??

 

 

 

 

Regards,

Muhammad Azeem Iqbal

Welding Inspector Aramco Approved

053110-8577/0554453626/0590071467

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/8e1f3a9f-2d27-44fa-b777-6a9e6ed119ddn%40googlegroups.com.




AVG logo

This email has been checked for viruses by AVG antivirus software.
www.avg.com


Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Re: [MW:14950] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

Dear All, I have been a CONSULTANT FOR such problem & my personal opinion is expressed as follow. I fully agree with views expressed so far. But bag to differ that " Code is a law, with engineering judgments. Hence the inspector has the rights to declare that the original HT was inadequate." Inspectors & total industry must resist the "REJECTION" . We as intellectual & having seniority must become practical. How the code will revise???. ANS.: One is experiments (Pure research) & second is such chances that gives opportunity to experiment !!! _______________________________________________________________________________________________ My understanding is that it is P1 material. In that case every pass normalizes the immediate bottom pass. Hence code requirement for P1 FOR MANDATORY SR is 32 mm & above thickness. SOLUTION:  In any case 0. After SR=PWHT no PTC testing is required as per code--Unless for low temp. vessels. That means code ...