Saturday, November 21, 2020

Re: [MW:31760] Facing crack in during overlay welding of Stellite 12 on Duplex material

Nickel barrier maybe required for stellite deposit on duplex steel. 
Vanchinath

On Fri, 20 Nov, 2020, 10:09 pm Srinivasan Jagannathan, <jsrisud@gmail.com> wrote:
Dear Suresh,
Grind the surface just before the deposition and try. This might be due to Chromium oxide which has already formed on the surface. Also slow cool by wrapping the entire job with an asbestos cloth.

Srinivasan  


On Fri, Nov 20, 2020 at 9:37 PM SURESH <qms.pjgpl@gmail.com> wrote:
Dear sir
While welding itself I am getting crack.

Ring is holded in the positioner by means of clamps at 90 degree and we are proceeding the welding.


Regards
Suresh

On Friday, 20 November 2020 at 16:47:34 UTC+5:30 JS wrote:
Dear Suresh

Are you getting the crack during the deposition? Or after the job is cooled?

Srinivasan

On Fri, Nov 20, 2020 at 3:16 PM SURESH <qms....@gmail.com> wrote:
Dear Experts
During welding of Duplex grade material we are facing crack on the weld metal as attached in the photo. Below is the detailed process for reference

Process: PTAW
Base Material: ASTM 182 Gr.F55
Consumable: Stellite 12 (Powder)
PreHeat: Nil
Interpass: <200*C
Current: 128 to 145
Gas: Ultra Pure ARGON
Job Size: OD544 X ID 472 X Thk 36mm
Welding: Overlay weld on OD Surface alone


We are welding deposition thickness of 3mm. So as per this we are doing welding of 2 layer with multi pass, On welding second layer we found crack. Can anyone suggest where it is went wrong and why this crack is propagated. Please advice

 

In First layer- Total of 12 weld pass

In second layer- Total of 12 weld pass



Regards

Suresh

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/8fd110ad-c422-4025-bf91-632d75b53a60n%40googlegroups.com.


--
J.SRINIVASAN
Mobile : 75501 82117



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b098ade0-08fa-49b1-8e31-afd4ad84e81an%40googlegroups.com.


--
J.SRINIVASAN
Mobile : 75501 82117



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKHQPVwPwqLG-p9X9Os89%3Dq7_pZ_AfauF4fEtVTj72J2GdpS5A%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CA%2B6Tn1LNHeaE8oU%3Dwb4jOtKL8EKUU2aFsYy6qxWEp0beMpg1Ng%40mail.gmail.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...