Cleaning prior to welding

To achieve low porosity levels for x-ray quality welds, it is important to understand the methods available for the effective removal of hydrocarbons and moisture from the weld area, and to incorporate the appropriate methods into the welding procedure. If these contaminants are present in the weld area during welding, they will produce hydrogen and significantly contribute to porosity problems.

When designing welding procedures intended to produce low levels of porosity, it is important to incorporate degreasing and oxide removal. Typically, you can achieve this through a combination of chemical cleaning and/or the use of solvents to remove hydrocarbons followed by stainless steel wire brushing to remove contaminated aluminum oxide.


so what is this methods in your point of view? 

Regards,
H.A 

On Tue, May 8, 2018 at 1:00 PM, George Dilintas <dilintas@gmail.com> wrote:

2018-05-08 9:11 GMT+03:00 'c sridhar' via Materials & Welding <materials-welding@googlegroups.com>:
Your photos clearly shows endless amount pores in the weld

The main cause for porosity in aluminum is hydrogen, which       has very high solubility in molten aluminum but very low            solubility in solid. Hydrogen gas is therefore evolved as the weld   pool solidifies. If the cooling rate is too high, the gas remains in      the metal in the form of porosity. Thus, any compound containing hydrogen and contaminating the filler wire or work surface can cause porosity.

Oil, moisture or other contaminants may be present on the        filler wire. In addition, the oxide layer of aluminum tends to get    hydrated and improper cleaning of the oxide layer immediately preceding welding could be a cause for porosity. Ensuring that     the plate is clean before welding and switching to clean, high   quality electrodes will reduce the likelihood of forming porosity.

The amount of porosity depends on how fast the weld pool  solidifies. Increasing the welding current and/or decreasing          the travel speed will increase the heat input, and help retard the cooling rate allowing gases to escape from the weld pool and  thereby reducing the risk of porosity.

Filler wires should ideally be kept in their packaging until      needed; wire that is left out ion open workshop conditions will absorb moisture into its oxide layer. It is advisable when welding aluminum to wipe each wire prior to use with a clean cloth dipped in acetone.
Pre heat the weld and HAZ area to mimnimum150 deg. C to eliminate hydrogen pores. Once you overcome it, the tests
will pass through.
Sridhar.


On Monday, 7 May, 2018, 4:16:16 PM IST, Hani Al Masry <hanyonalfy@gmail.com> wrote:


Dear experts 

regarding A/M Subject kindly advice why the PQR Test had been failed two times even this WPS/PQR Approved before and we just tried to copy it 

all welders 2 times failed in root bend / tension some times not reach 250 MPA as required  (2 root bend + 2 root face + 2 tensile testing are required)

the lab said first time there are porosity
and inclusions but even 2nd test was failed  (attached photos for your reference) 

BASE METAL       :  AA 5083 H 321  
FILLER METAL       :  ER 5356  
Joint Preparation: -              Single V CPJ

Weld Layer

WELDING PROCESS

WELDING POSITION / DIRECTION

ELECTRODE(S)

GAS SHIELD

GAS FLOW RATE

lit/min.

AMPS

VOLTS

WELDING SPEED mm./min.

FLUX

WFS

M/Min.

Mode of Metal transfer for MAW

SIZE

mm

TRADE NAME

POLARITY

1

GMAW

3G

1.2

AUTO ROD 5356

DCEP

ARGON 99.99%

15-25

120-180

18-26

12-20

NA

8.5

Pulse transfer

2

GMAW

3G

1.2

AUTO ROD 5356

DCEP

ARGON 99.99%

15-25

120-180

18-26

120 - 140

NA

8.5

Pulse transfer

Back weld

GMAW

3G

1.2

AUTO ROD 5356

DCEP

ARGON 99.99%

15-25

120-180

18-26

100 - 110

NA

8.5

Pulse transfer









--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...