--Dear Pradip:
Delayed cracking is caused by Hydrogen embrittlement. They are typically transverse to the weld but in your case it runs with the weld, which is unusual. By close observation, the crack mostly offsets the centerline and near HAZ. Because you mentioned that the joint preparation has "little beveling", I am wondering if the crack originates from under the surface where lack of fusion occurred at the fusion line.
To solve the problem, you may consider the following approach:
1. After welding and weld metal cooled to room temperature (to finish Martensitic transformation), immediately do PWHT within 5 ~ 6 hours.
2. If this is not feasible, conduct a Hydrogen baking heat treatment at 600 F ~ 650 F for 1 hour.
3. Increase the bevel angle or train and enhance the welder's skill to avoid Lack of Fusion problem
Thanks!
Feng Lu, Ph.D., NDE Level III
Metallurgy and Welding Engineer
Zachry Industrial, Inc.
3600 West Sam Houston Pkwy Southluf@zachrygroup.com
Office: 713.979.2648
Cell: 512 797 5777
www.ZachryGroup.comThis e-mail may contain confidential and privileged material for the sole use of the intended recipient. Any review, use, distribution or disclosure by others is strictly prohibited. If you are not the intended recipient (or authorized to receive for the recipient), please contact the sender by reply e-mail and delete all copies of this message.
From: materials-welding@
googlegroups.com [mailto:materials-welding@googlegroups.com ] On Behalf Of pradip kumar Sil
Sent: Sunday, February 11, 2018 4:38 AM
To: materials-welding <materials-welding@googlegroups.com >
Subject: [MW:27331] P-22 plate welding ...6-MM plate
Dear Everybody,
We are doing P-22 plate welding, thickness is 6 mm with E-9018B3 ( Dia 2.5 mm) electrode. Preheat is 150 to 200 degree centigrade with little beveling. Site is near the sea area.
We found lot of delayed crack generally after 12 hours. Crack is coming middle of the weldment.
Can anybody inform me cause & corrective action for the same.
Pic attached for your ready reference.
Thanks in advance.
Regards,
--
https://secure-web.cisco.com/1ooeDbhv3BPAMRKQvZje5BpOTSLbED rOt6clzNi9B_ZUOl_ YtqVs0vXuMokwNj4rTeKHWWwQiVIhE NXiATpcZDadEDiXsf0hZincHJb9PPT OyH0Bvhoq3OGa1xwnOiwr4kFpIzQxV BQ5RxHXYrWVZu6tOugiYyKNNkj0YvK A9JRXAm9SxxX7c-BM2U_ w87QoACYYvW22yXG0V9w11dAnzgXui HGkxt0MabiS127GlrD76K98a2uv3yA dZf90POrUVsCGRKzIWcCHaL1_ oE6VZk9Q8-mVxOVGxLm0h15gZf_ 499pXJKi8TAv_uHhsc4k_i_ UJfBaULOQ7NxI8X95UIIg/https% 3A%2F%2Fmaterials-welding. blogspot.com%2F 
https://secure-web.cisco.com/1qduLuIrqt8RsNdxRyXgE0BokLmk26 NhL8khuqh2Y2hZeOxDyNJdab- grM8hcofjy7OPKpKS30EJccCPW5-- p_ 5S2fVEPCHo5bPmXGJG8Sb85r3PKkmV cEqVGdrHQDFazeWzkN1XIfRyWPYOz1 TZcXDBP9If9wJySyk1vluoF- 8WFwdh9Q6FPDvhtKPNTURHDrEYs9Cl nO-w- bBXVMPNYbeyAghEsYKUYlgeGvefefB IdgkUWCZAzZjkq1hnY4dEQljDW3q_ fEVVAswsst0Xr0XjVz9I5lU1_-_ U8RGvfKJSiWIQIQE3tySqb1hEtEee6 Nz56WE4zjLqVM1F-VGmXvg/https% 3A%2F%2Fwww.linkedin.com% 2Fgroups%2F122787 
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com .
Visit this group at https://secure-web.cisco.com/16bhCpksvjRMYc1qvdIMvnu7v0DpC1 .GLplubvyw61H3un6TBlccvAAnSt880 JNNAELwfG8YKr1Ov1DGtX8cKljrUJG qVfcdxBe3NTuyVOGhrlCoSYtp4ypfY qRWF5HE-F509n0NB_EUzZEfz3_ Jdl6oRMWDYoLO941JnVlIyeBRQSwlV C3dIfFGrYLn0XKlzeB-6b5_ jUheEIsLfo0ywjfdqmAE7yDe_ VeJrXR2WDUgwHp3ImgZp6Z3HZtP9jB x-o1e4tnf1P5c15Hzp- pq1lpWD64r9kW6DjeRRL6K- QQFFYidIS9rA7Vcsxkvb_ NoDe4ng24bJN0rPdbc2ldDzcSw/ https%3A%2F%2Fgroups.google. com%2Fgroup%2Fmaterials- welding 
For more options, visit https://secure-web.cisco.com/1U3Son64DzOOm5-LMh_ .LExhSItYs4yBqwGyhwXhIgKYNMuM_ nM5YrJSzJX8mgK855E9UOxaMjmS8nD M0dEx-Mt3zldfKLy4_ KNd0antFC6NtQCjP59yXEHtYfDccKW m5bUrKtdZ9UumC-LQi_ jXbcFxYOeydZBfMbogI57BImguAw3r RjhLBx-vC_iirbTcwRC_ dgI2WqJtkscyGqpDehVJvNcBxht6kA c48LFulNa5TB3XETYt9zyfiUl4T- Hn4gWlH7Bsg9qWGEJV6F8_ eF0lPICo7qekBnZGSfzOhi8_ 88jYeTs2IjfwFElvFMDHARliSQ_ dlrn95mcyC6W32jbw/https%3A%2F% 2Fgroups.google.com%2Fd% 2Foptout 
https://materials-welding.blogspot.com/ 
https://www.linkedin.com/groups/122787 
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com .
Visit this group at https://groups.google.com/group/materials-welding .
For more options, visit https://groups.google.com/d/optout .
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments