Delayed cracking is caused by Hydrogen embrittlement.  They are typically transverse to the weld but in your case it runs with the weld, which is unusual.   By close observation, the crack mostly offsets the centerline and near HAZ.  Because you mentioned that the joint preparation has "little beveling", I am wondering if the crack originates from under the surface where lack of fusion occurred at the fusion line.

 

To solve the problem, you may consider the following approach:

 

1.       After welding and weld metal cooled to room temperature (to finish Martensitic transformation), immediately do PWHT within  5 ~ 6 hours.

2.       If this is not feasible, conduct a Hydrogen baking heat treatment at 600 F ~ 650 F for 1 hour.

3.       Increase the bevel angle or train and enhance the welder's skill to avoid Lack of Fusion problem

 

Thanks!

 

 

Feng Lu, Ph.D., NDE Level III
Metallurgy and Welding Engineer

Zachry Industrial, Inc.
3600 West Sam Houston Pkwy South

Suite 200

Houston, TX 77042

luf@zachrygroup.com
Office: 713.979.2648
Cell: 512 797 5777
www.ZachryGroup.com

This e-mail may contain confidential and privileged material for the sole use of the intended recipient. Any review, use, distribution or disclosure by others is strictly prohibited. If you are not the intended recipient (or authorized to receive for the recipient), please contact the sender by reply e-mail and delete all copies of this message.

 

 

 

 

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of pradip kumar Sil
Sent: Sunday, February 11, 2018 4:38 AM
To: materials-welding <materials-welding@googlegroups.com>
Subject: [MW:27331] P-22 plate welding ...6-MM plate

 

Dear Everybody,

 

We are doing  P-22 plate welding, thickness is 6 mm with E-9018B3 ( Dia 2.5 mm) electrode. Preheat is 150 to 200 degree centigrade with little beveling. Site is near the sea area.

 

We found lot of delayed crack  generally after 12 hours. Crack is coming middle of the weldment.

 

Can anybody inform me cause & corrective action for the same. 

 

Pic attached for your ready reference.

 

Thanks in advance.

Regards,

 

--
https://secure-web.cisco.com/1ooeDbhv3BPAMRKQvZje5BpOTSLbEDrOt6clzNi9B_ZUOl_YtqVs0vXuMokwNj4rTeKHWWwQiVIhENXiATpcZDadEDiXsf0hZincHJb9PPTOyH0Bvhoq3OGa1xwnOiwr4kFpIzQxVBQ5RxHXYrWVZu6tOugiYyKNNkj0YvKA9JRXAm9SxxX7c-BM2U_w87QoACYYvW22yXG0V9w11dAnzgXuiHGkxt0MabiS127GlrD76K98a2uv3yAdZf90POrUVsCGRKzIWcCHaL1_oE6VZk9Q8-mVxOVGxLm0h15gZf_499pXJKi8TAv_uHhsc4k_i_UJfBaULOQ7NxI8X95UIIg/https%3A%2F%2Fmaterials-welding.blogspot.com%2F
https://secure-web.cisco.com/1qduLuIrqt8RsNdxRyXgE0BokLmk26NhL8khuqh2Y2hZeOxDyNJdab-grM8hcofjy7OPKpKS30EJccCPW5--p_5S2fVEPCHo5bPmXGJG8Sb85r3PKkmVcEqVGdrHQDFazeWzkN1XIfRyWPYOz1TZcXDBP9If9wJySyk1vluoF-8WFwdh9Q6FPDvhtKPNTURHDrEYs9ClnO-w-bBXVMPNYbeyAghEsYKUYlgeGvefefBIdgkUWCZAzZjkq1hnY4dEQljDW3q_fEVVAswsst0Xr0XjVz9I5lU1_-_U8RGvfKJSiWIQIQE3tySqb1hEtEee6Nz56WE4zjLqVM1F-VGmXvg/https%3A%2F%2Fwww.linkedin.com%2Fgroups%2F122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://secure-web.cisco.com/16bhCpksvjRMYc1qvdIMvnu7v0DpC1GLplubvyw61H3un6TBlccvAAnSt880JNNAELwfG8YKr1Ov1DGtX8cKljrUJGqVfcdxBe3NTuyVOGhrlCoSYtp4ypfYqRWF5HE-F509n0NB_EUzZEfz3_Jdl6oRMWDYoLO941JnVlIyeBRQSwlVC3dIfFGrYLn0XKlzeB-6b5_jUheEIsLfo0ywjfdqmAE7yDe_VeJrXR2WDUgwHp3ImgZp6Z3HZtP9jBx-o1e4tnf1P5c15Hzp-pq1lpWD64r9kW6DjeRRL6K-QQFFYidIS9rA7Vcsxkvb_NoDe4ng24bJN0rPdbc2ldDzcSw/https%3A%2F%2Fgroups.google.com%2Fgroup%2Fmaterials-welding.
For more options, visit https://secure-web.cisco.com/1U3Son64DzOOm5-LMh_LExhSItYs4yBqwGyhwXhIgKYNMuM_nM5YrJSzJX8mgK855E9UOxaMjmS8nDM0dEx-Mt3zldfKLy4_KNd0antFC6NtQCjP59yXEHtYfDccKWm5bUrKtdZ9UumC-LQi_jXbcFxYOeydZBfMbogI57BImguAw3rRjhLBx-vC_iirbTcwRC_dgI2WqJtkscyGqpDehVJvNcBxht6kAc48LFulNa5TB3XETYt9zyfiUl4T-Hn4gWlH7Bsg9qWGEJV6F8_eF0lPICo7qekBnZGSfzOhi8_88jYeTs2IjfwFElvFMDHARliSQ_dlrn95mcyC6W32jbw/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...