the corrosion property will deteriorate to some extent based on the PWHT control,
as SS 347 is stablized one deterioration will be limited to some extent
WPS shall be qualified on cladded plate with PWHT and corrosion test on cladded area after PWHT to ensure corrosion property
On Sat, Jun 11, 2016 at 7:08 PM, 'Biplab Pal' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Dear Experts,--We have the Cladded Pipe of ASTM A335 Gr P11 (9.3 mm to 25 mm) with internally cladded with SS347 (3mm).We need to weld the Pipe Support with the pipes.Our pipe support is P11 grade and the WPS is qualified with PWHT @740 for minimum 2 hours.If we do PWHT is it going to effect the SS cladding? is there any corrosion issue.We need your kind advice.--Thanks & Regards
Biplab Pal
Welding InspectorE-mail: biplab.mech@gmail.com
Information in this email and any attachments is confidential and intended solely for the use of the individual(s) to whom it is addressed or otherwise directed. Please note that any views or opinions presented in this email are solely those of the author and do not necessarily represent those of the Company. Finally, the recipient should check this email and any attachments for the presence of viruses. Myself accepts no liability for any damage caused by any virus transmitted by this email.
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFnzQg2_KsLhkjO679d_%3DfmBGrk_LD1J_yRKUETXr%2B2MP_OCVg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
Thanks and Regards
M.Sathyanarayanan
M.Sathyanarayanan
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzo-ktHk8oohnor7wFkxJNHZnMnqq_bgWRJT_OUjf9%2BchTBAQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
Comments