Skip to main content

RE: [MW:24742] RE: 24723] welding filler metal for SS321

This an Air Cooler, and the operating temperature is +350C.


Date: Mon, 25 Apr 2016 00:04:41 -0400
Subject: Re: [MW:24739] RE: 24723] welding filler metal for SS321
From: pgoswami@quickclic.net
To: materials-welding@googlegroups.com
CC: pgoswami@quickclic.net

What's the process fluid and the design temperature? 

-------- Original message --------
From: Himan Nikdin <himan.nikdin@outlook.com>
Date: 2016-04-24 11:26 PM (GMT-05:00)
To: materials-welding@googlegroups.com
Subject: [MW:24734] RE: 24723] welding filler metal for SS321


Dear Pradip

Since the operating temperature is below 400C, I think the E308LSi can be a good choice, Are you agree?

Regards,
Himan

From: pgoswami@quickclic.net
To: materials-welding@googlegroups.com
CC: himan.nikdin@outlook.com
Subject: RE: 24723] welding filler metal for SS321
Date: Wed, 20 Apr 2016 11:05:35 -0400

Hi Himan,

 

What's proposed by ESAB is not correct. Please seethe two attachments showing highlighted texts. S.S 321 is a Titanium stabilized steel. Hence the matching weld metals also  shall be  stabilized.

 

Titanium gets oxidized fast when it's added through coating.  Hence other stabilizers such as Nb has to be added to the weld puddle to provide the stabilized weld metal as well as provide the high temperature Creep Properties. Thus 347 electrodes/fillers are the only solution.

 

Hope it clears your doubt.

 

Thanks.

 

 

Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist & Consultant.
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgoswami@quickclic.net

pradip.goswami@gmail.com

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Himan Nikdin
Sent: Tuesday, April 19, 2016 11:21 PM
To: materials-welding@googlegroups.com
Subject: [MW:24723] welding filler metal for SS321

 

Dear Experts

 

Refer to API582 table A-2 proposed filer to weld SS321 to SS321 is E347-XX/ER-347 but some manufacturers such as ESAB propose E/ER-308LSi to this base material (SS321 to SS321) operating temperature is +350 C,

would you please advise in this issue.

 

Regards,

H.Nikdin


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/BLU180-W823AE7188B8126FC9E22999E6D0%40phx.gbl.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/hsb2r0xdf0r3yp6g1is6tv9l.1461557081654%40email.android.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...