Hi Mohit,
             As per any standard, you cannot perform tensile test by pressing tube ends. You have plug the ends with length as specified in standard.

2016-04-11 11:23 GMT+04:00 Mohit Aggarwal <aggarwalmohit05@gmail.com>:

Dear Sir,

Greetings of the day!

I have one query, I have done Tensile test for full  Pipe specimen OD 25.7mm and thk 2.1 mm material SS 304L according to EN standard by calculating gauge length by consideration the OD of pipe with formula 5.65 x square root of Area which is coming 130 mm rounded off . In UTM machine I have select hollow pipe section and tensile strength is coming automatically with these settings.
But elongation is coming 32% and minimum required is 40%. We have done test by pressing the pipe ends.

Kindly let me know where is actual problem can oocurs.

I will be thankful to you.

Best Regards,
Mohit Aggarwal

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALTezPPPV9P8U4mzjp%2BV_6c4q4mCQxNZnpPEoykdZdj0WZE3EA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.



--
Regards,
Mr. Harish.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAE4SttEDg-1VntZxV64Xj%3DtQef9%2BD1DJ1Yd%3Dugmm5snpqomeGw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35738] ASME IX WPS Qualification Query: GTAW + FCAW with Multiple PQRs

Dear Welding Experts, I'm currently preparing a Welding Procedure Specification (WPS) and have encountered a request to qualify a GTAW +...