Skip to main content

Re: [MW:24647] EN 10025 S275JR

Dear Salhi,
EN S275JR material not listed in QW 422  
So, it was called as unassigned P.no

You have the WPS for A106Gr.B - you cant use for EN SA275JR material

You have to make a new PQR using the material EN S275JR

Pls refer to the para QW-424

Best Regards,
Chandra

On 07-Apr-2016, at 12:14 PM, Demir Alp <demiralp85@gmail.com> wrote:

Dear Mr. Alagarsamy & Mr Salhi ;

Please correct me if i am wrong , but as per QW-211, a WPS qualified by pipe covers plate and vice versa.

Please see the extracted ASME Sec IX article in the attachment.



On Wednesday, April 15, 2015 at 8:29:45 AM UTC+5, Alagarsamy wrote:
Dear Naveen,
 
                  As per Mr. Salhi said ,its correct that material equivalent.And Also i give the additional information

 

This is common carbon steel plate in S235JR, S235J0 and S235J2 steel grade. Heat analysis shall be used to determine the required chemical composition for carbon. Manganese, phosphorus, sulfur, silicon, and copper. Tensile strength, yield strength, and elongation shall be evaluated using tension test.

 

S symbol for structural steel 
275 indication of the min specified yield strength for thickness of under 16mm.
JR symbol 20 temperature impact test.
J0 symbol 0 temperature impact test

J2 symbol -20 temperature impact test

 

 

S275JR, S275J0 and S275j2 steel is a structural steel grade which be used in riveted, bolted, or welded construction of bridges and buildings.

 

For more information of S275j2 steel, please refer them in following.

 

The Chemical is max composition of product analysis:

 

Grade

C %

Si %

Mn %

P %

S %

N %

Cu %

S275J2

0.210

-

1.600

0.035

0.035

-

0.060

 

The mechanical properties steel plate

 

Grade

Thickness(mm)

Min Yield (Mpa)

Tensile(MPa)

Elongation(%)

Min Impact Energy

S275j2

8mm-100mm

275Mpa

430-560Mpa

21-23%

-20

27J

101mm-200mm

225-235Mpa

400-540Mpa

19%

-20

27J

201mm-400mm

215Mpa

380-540Mpa

18%

-20

27J

The min impact energy is longitudinal energy




2.You cant use same WPS,because this material plate type.You have WPS for pipe material.You can follow that WPS format as per your site using standard


On Mon, Apr 13, 2015 at 11:32 AM, 'raouf salhi' via Materials & Welding <material...@googlegroups.com> wrote:
Dear sir ;

1 - The EN S275 JR is an europeen normalisation ( S mean structure , 275 is the yield strength , JR means 27 J at 20 °c for impact test) , the equivalent in ASME is the SA 572 ( p number 1).

2- they have the same P number but  A106 is a  pipe ( usually welded GTAW / SMAW) and the EN S275 JR is a plate usually welded only SMAW ( with backing ).
I don't think that you can use the same WPS.

3- no it's not correct

Regards
 
SALHI Raouf
QA/QC Engineer

Tel: Morocco +212628979891
      Tunisia +21621458258



Le Lundi 13 avril 2015 4h23, Naveen Raj <mecna...@gmail.com> a écrit :


Dear All,

1. Can anyone tell me what is the P.no for EN 10025 S275JR

    I searched in ASME IX but i didnt find.

2. I have WPS for CS (SA106) material, can i use this WPS for welding Mild steel (EN 10025 S275JR)

    looking for reply from u guys......

3. WPS shall be for only the material which they are going to weld and not to all equivalent material as mentioned in the Material specification description of WPS.

     is it correct????
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/a6e45df1-e3fb-4ddb-ad98-619f665411a5%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit
...

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/7c3025a4-2135-4047-a849-98a36d1c8282%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
<qw-211.JPG>

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...