Skip to main content

[MW:24725] RE: 24723] welding filler metal for SS321

Hi Himan,

 

What’s proposed by ESAB is not correct. Please seethe two attachments showing highlighted texts. S.S 321 is a Titanium stabilized steel. Hence the matching weld metals also  shall be  stabilized.

 

Titanium gets oxidized fast when it’s added through coating.  Hence other stabilizers such as Nb has to be added to the weld puddle to provide the stabilized weld metal as well as provide the high temperature Creep Properties. Thus 347 electrodes/fillers are the only solution.

 

Hope it clears your doubt.

 

Thanks.

 

 

Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist & Consultant.
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgoswami@quickclic.net

pradip.goswami@gmail.com

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Himan Nikdin
Sent: Tuesday, April 19, 2016 11:21 PM
To: materials-welding@googlegroups.com
Subject: [MW:24723] welding filler metal for SS321

 

Dear Experts

 

Refer to API582 table A-2 proposed filer to weld SS321 to SS321 is E347-XX/ER-347 but some manufacturers such as ESAB propose E/ER-308LSi to this base material (SS321 to SS321) operating temperature is +350 C,

would you please advise in this issue.

 

Regards,

H.Nikdin

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...