Dear sir,
Please check usage of wrap around bend instead of roller bend.
Regards,
Maulik
Welding engg.
L&T, Hazira
Dear friend,Before any recommendation about welding note that for some material grades like yours, with low elongation (in your case 16% min requirement), the laboratory has to care about bending mandrel diameter. You could check QW-466.1 for better understanding of proper jig dimension.Regards--On Thu, Nov 27, 2014 at 5:35 PM, Mohd Azam <azam1976@gmail.com> wrote:--Dear Experts,
We are facing the problem bend test failure for Aluminum TIG welding. Its failing for HAZ and getting crack for transverse face bend, Root bend sample (10 mm thickness as welded sample). Pls give some details to bend for aluminum sample, If anyone have experience in aluminum TIG welding. Pls share your experience and provide some welding guideline. What could be the reason of failure or the bend testing requirement for Aluminum welding.
Process: GTAW
Filler: ER5183
Base Material: ASME SB209 Grade 5083-O
Code: ASME IX
Thickness: 10 mm
Thanks & Regards,
Mohd. Azam
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
--M. Shokri ArfaeiISA-ISTS - Metallurgy Lab. ManagerASNT NDT Level IIIInternational Welding EngineerTel.: +98 21 66282127Fax: +98 21 66282779Mob.:+98 912 1394023
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
Comments