Hi
 
You have to use ER 110S-G MIG wire.
While welding strictly maintain an interpass temp. of @ 200 degrees C max., weld with higher travel speeds to reduce heat input inorder to get better properties.
 
Regards
 
Prem Nautiyal

--- On Mon, 10/1/12, G Sreenivas Rao <gsrinivasg3@gmail.com> wrote:

From: G Sreenivas Rao <gsrinivasg3@gmail.com>
Subject: [MW:15434] suitable welding MIG wire for Weldox 700
To: materials-welding@googlegroups.com
Date: Monday, October 1, 2012, 9:39 AM

Dear all
Hello to all and  can any body suggest tyhe Mig wire for weldox700
materail, we are the manufacuturer of Industrial centrifugal fans and
we require above mentioned suggestion.
we are used MIG wire, ER100s,  and ER100S, but we dint get required
tensile strength.


Regards

G.Sreenivas Rao
Turbovent Industries Pvt. Ltd.
+91 9441511368

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

No comments:

[MW:35346] Cast-iron welding

Any advice for cast iron welding Sent from Yahoo Mail for iPhone