Re: [MW:15763] welding procedure for 12Cr1MoVG

Dear Friend,
                    12Cr1MoV is a Chinese material.
Material Chemical composition
C Mn Si Cr Mo V Ni Ti B W Nb Cu S P
0.08-0.15 0.4-0.7 0.17-0.37 0.3-0.6 0.25-0.35 0.15-0.30 - - - ≤0.035 ≤0.035
 
Tensile strength 440MPa
Yield strength 225Mpa

Electrode Selection ASME Sec IIC  Filler Wire SFA5.28

AWS  UNS  C  Mn  Si  P S Ni Cr Mo V Ti Zr Al Cu Other elements Total
ER80S-B2  K20900  0.07-0.12  0.40–0.70  0.40–0.70  0.025 0.025 0.2  1.20–1.50  0.40–0.65  —  —  —  —  0.35 0.5

 Tensile  strength 550MPA
Yield Strength  470MPA

Electrode SFA5.5

AWS  UNS  C  Mn  Si  P S Ni Cr Mo
E8018-B1  W51018  0.05–0.12  0.9 0.6 0.03 0.03 —  0.4—0.65 0.4—0.65

Tensile  strength 550MPA
Yield Strength  460MPA

Company:D&H
Filler wire Brand:FCr-MO1
Electrode Brand:Chromotherm

On Thu, Oct 18, 2012 at 8:35 PM, Roy Liu <standardliu@hotmail.com> wrote:
Hi, friend!
exactly, this is a Chinese material name. 12Cr1MoVG is pearlitic heat resistance steel, similar with 1.25Cr-0.5Mo, but plus V. It is suitable for Boiler or High Temp./Pressure Vessel in Thermal Power Industry.
you may buy filler metals from China.
 
Bohler Welding Could Offer You The Best Solution:
1, SMAW: BOHLER FOX DCMV / FOX DMV 83 Kb
2, GTAW/GMAW: BOHLER DMV 83-IG
 
 
Regards
 
Roy
Bohler Welding China Office
 
 
 
-----原始邮件-----
From: HAREESH K V
Sent: Thursday, October 11, 2012 11:33 PM
Subject: [MW:15574] welding procedure for 12Cr1MoVG
 
Dear experts,
 
please help on this topic. I need welding procedure for 12Cr1MoVg.
This is as per chinese standard which contains 1.2Cr. This contains
Vanedium also. Which electrode to be used for welding?
Please help me.
 
----------------------
Hareesh K V
NeoStructo Construction Ltd.
91-9447625012
 
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...