Dear Chintu:

Mo is very critical here,
Since 316 or 2205 are being used because of their Mo content (for salt water or pitting corrosion resistance), so you must make sure that your weld has that minimum amount of Mo as in 316 (to match "cheaper" base metal in this joint).

2205: Mo 3%
316 : Mo 2-3%
E309L-Mo : Mo 2.7%

So as Mr.
Ahmed Osman mentioned, you may use E2209 or E309LMo (whichever you choose, Mo content is acceptable)

You have to know how to use De-Long diagram to be able to accurately select a filler metal for such dissimilar welds
.

Regards
Ramin  Kondori
   QC/Welding Engineer 
         IWE AT 0070
   



On Fri, Aug 19, 2011 at 4:30 PM, Morin, Darcy (Bantrel Management Services) <MorinD@bantrelmanagementservices.com> wrote:
Here is the chart from API which deals with SS mismatches. 
Darcy Morin
 
 
 



-----Original Message-----
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Ahmed osman
Sent: Friday, August 19, 2011 2:59 AM
To: materials-welding@googlegroups.com
Subject: [MW:12273] FW: 11108] DUPLEX S.S. (S.S. 2205) TO AUSTENITIC S.S. (Grade 316L) welding.

U can use E2209 or E309MoL
Ahmed Osman
Sr Q.C. Eng.

-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of CHINTUKUMAR GANDHI
Sent: Saturday, May 21, 2011 12:21 PM
To: materials-welding@googlegroups.com
Subject: [MW:11108] DUPLEX S.S. (S.S. 2205) TO AUSTENITIC S.S. (Grade 316L) welding.

Dear Experts,

I come across with very strange welding combination. That is Duplex stainless steel to ausatenitic steel welding. Here Flange is SS 316 L & pipe is duplex stainless steel (2205).

plz guide me abt which filler wire I should use?  & which good engineering practises should adopt during welding.

Chintu Gandhi

Welding Engineer 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

This e-mail and any attachments may contain confidential and
privileged information. If you are not the intended recipient,
please notify the sender immediately by return e-mail, delete
this e-mail and destroy any copies.

Any dissemination or use of this information by a person other
than the intended recipient is unauthorized and may be illegal.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...