If E410 is used to weld SS410 then how are the distortion stresses in the weld addressed? (considering preheat 250DegC and post heat 350DegC X 3Hrs)

On Sun, Mar 6, 2011 at 5:18 PM, kannayeram gnanapandithan <kgpandithan@gmail.com> wrote:
If Strengh is not criteria, austenetic filler is being used ,otherwise matching filler only


On Sun, Mar 6, 2011 at 7:26 AM, narisepalli venkateswara prasad <nvprasad1968@gmail.com> wrote:
Dear Gerald,
 
you can use E 309L for welding of  TP 409 SS and it is austenitic is better choise than ferritic filler materia

 Please find  here with the useful article regarding this.
 
Regards
 
N.V. PRASAD
SR. WELDING ENGINEER
KHARAFINATIONAL, UAE.
 
 
On Thu, Mar 3, 2011 at 3:12 PM, James, GeraldJayakumar <GeraldJayakumar_James@fwuk.fwc.com> wrote:

GTAW : ER409/ER409Nb (SFA 5.9)

SMAW : E409Nb (SFA 5.4)

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Martin Prad
Sent: Thursday, March 03, 2011 4:09 PM
To: materials-welding@googlegroups.com
Subject: [MW:10116] welding of ASTM A240 type 409 S40900 steel plate

 

Hi,


 
Could you please advise which consumable/wire can be used for welding of this type of steel?
 
regards,
Martin.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


Confidentiality Notice

This communication and the information it contains:-
(a) Is intended for the person(s) or organisation(s) named above and for no other person(s) or organisation(s).
(b) May be confidential, legally privileged and protected in law. Unauthorised use, copying or disclosure of any of it may be unlawful. If you have received this communication in error, please contact us immediately by email at Postmaster@fwuk.fwc.com.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34919] Welder qualification certificate

Dear All     anyone can share a format for welder certificate and card format        Thanks & Best Regards Saleem manhappulath Mob:+9665...