can you pls provide UOP para( Extract) which states --
Tempering temp shall be 28 °C higher than PWHT temp)
Regards
On Thu, Dec 30, 2010 at 12:58 PM, Bathula Raghuram (Mumbai - PIPING) <R.Bathula@ticb.com> wrote:
IBR regulation 282a: states tempering temperature for P11 shall be 620-660 °C and for P22 it shall be between 650-700 °C.
Whereas Minimum PWHT temperature for B31.3 piping is 704 °C, when we restrict the min tempering temp to (e.g. 730 °C), forging vendors are denying to meet the requirement (e.g. welded valves), quoting IBR regulation 282a.
However there is a note at the end "The tempering temperature may be varied by the Inspecting Authority to suit the steel being tempered".
My question is had anybody approached in the past and able to convince IBR for higher tempering temperatures?
Q: how forging vendors are meeting this requirement when PWHT temperature shouldn't exceed tempering temperature (for e.g. UOP states tempering temp shall be 28 °C higher than PWHT temp)
Filtered by Hosted Filtering
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Comments