RE: [MW:8997] Combination of PQR for WPS

QW-200.4 (a) allows you to combine these two PQR's to support a single WPS.  In such a case the WPS will be restricted to the minimum range qualified by the PQR base metals (per QW-451);  i.e. the intersection of the two individual qualified ranges.   Therefore, your WPS would allow the following (assuming no impact requirements):

 

Qualified base metal range:  5mm to 12mm  ( 1.5mm < T1 < 12mm, 5mm < T2 < 30mm )

Maximum Qualified GTAW deposit:  12mm

Maximum qualified SMAW deposit:  12mm

 

 

REF:  (from HSB site)  Interpretations – File No. BC-80-628, no interpretation number

 

Question (2): A WPS is being written for groove welding of pipe to utilize a GTAW root pass and SMAW fill. A previously qualified PQR welded on a ¼ in. thick test plate using GTAW and a previously qualified PQR welded on a 3/8 in. thick test plate using SMAW are to be used to support the combination WPS. What are the maximum thickness ranges of the combination WPS?

Reply (2): Based on Question (2), the deposited weld metal thickness range for the GTAW is 1/16 in. through ½ in. and for the SMAW is 1/16 in. through ¾ in. The base metal thickness range for the combination WPS is 1/16 in. through ½ in.

 

Ref. also, HSB topic Specific Code FAQs:

 

Q: Is it possible to apply two separately qualified WPS's to the same joint in combination without qualification of a combined PQR?

A: Per QW-200.4, it is acceptable to apply both WPS's to the same joint without further qualification. The deposited weld metal qualification ranges may be "stacked", allowing the application of the maximum qualified thickness of deposited weld metal for each WPS/process in a single joint. However, the user is cautioned that the maximum base metal thickness qualified for the most limiting WPS must be applied. The base metal thickness ranges cannot be "stacked" to qualify for a greater thickness in combination.

(In my opinion the italicized section also applies to the minimum qualified thickness as well as the maximum)

If impacts were required, since there would be no intersection of qualified base metal thickness, one could not combine the two PQR's to support a valid WPS.  New PQR(s) would have to be performed.

 

QW-200.4(b) is an exception to the general rules for root pass process qualified with a PQR with base metal thickness > 13mm, and a second PQR for a fill process qualified with a base metal thickness greater than the base metal thickness used with the root pass PQR.  With the enquirers conditions, QW-200.4(b) does  not apply as both PQRs would have to have been performed on material thickness greater than 13mm which is not the case.  One example of an acceptable combination would be PQR 1 –13mm thick base metal w/ GTAW root (for the purpose of example say 6mm deposit thickness, t) combined with PQR 2:  38mm base metal thickness welded completely by SAW

These conditions would result in a combined WPS such as:

 

Qualified base metal range:  5mm to 200mm

Qualified maximum GTAW deposit thickness:  12mm

Qualified maximum SAW deposit thickness:  200mm

 

Hope this helps - John

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of praveen alavandar
Sent: Wednesday, December 29, 2010 5:35 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:8984] Combination of PQR for WPS

 

manpreet,

 

you still cannot combine both these PQRs, you should either use PQR 1 or PQR 2.

 

Regards,

 

Praveen

--- On Wed, 12/29/10, manpreet <manpreetsin88@rediffmail.com> wrote:


From: manpreet <manpreetsin88@rediffmail.com>
Subject: Re: [MW:8979] Combination of PQR for WPS
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Date: Wednesday, December 29, 2010, 3:25 PM

Dear Pravin,

Thanks for your valuable feedback.

I did consider QW-200.4(b) and wanted further calrification so i raised this point,
now i would present actual ranges, no impact required

PQR 1-  1.5mm to 12mm
PQR 2-   5mm to 30mm 

Combined:- 5mm to 12mm, is it ok now?

Regards
Manpreet Singh





On Wed, 29 Dec 2010 13:32:29 , praveen alavandar <praveenakds@yahoo.com> wrote

Manpreet,

 

You cannot support combining these two PQR's to prepare a WPS having a wide range from 1.5mm to 30mm, you are deviating from the clause QW-200.4(b) of ASME Sec.IX.

see below.

 

"For GTAW, SMAW, GMAW, PAW, and SAW, or combinations of these processes, a PQR for a process recording a test coupon that was at least 12 in. (13 mm) thick may be combined with one or more other PQRs recording another welding process and any greater base metal thickness. In this case, the process recorded on the first PQR may be used to deposit the root layers using the process(es) recorded on that PQR up to 2t (for shortcircuiting type of GMAW, see QW-404.32) in thickness on base metal of the maximum thickness qualified by the other PQR(s) used to support the WPS. The requirements of Note (1) of tables QW-451.1 and QW-451.2 shall apply."

 

So you will have,

 

for PQR 1 : WPS range : 1.5mm to 12mm (Without impact) & 2.5mm to 12mm (With impact) assuming you dont do a PWHT above the upper transformation temperature.

 

For PQR 2: WPS range : 5mm to 30mm (Without impact) & 15mm to 30mm (With impact)

 

Regards,

 

Praveen



--- On Wed, 12/29/10, Bathula Raghuram (Mumbai - PIPING) <R.Bathula@ticb.com> wrote:


From: Bathula Raghuram (Mumbai - PIPING) <R.Bathula@ticb.com>
Subject: RE: [MW:8975] Combination of PQR for WPS
To: "materials-welding" <materials-welding@googlegroups.com>
Date: Wednesday, December 29, 2010, 12:57 PM

5-12mm w/o impact, else 6-12mm

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of manpreet
Sent: Wednesday, December 29, 2010 12:03 PM
To: materials-welding
Subject: [MW:8974] Combination of PQR for WPS

 

Dear All,

Procedure qualification as per ASME sec ix,

I have 2 PQR:-
                        *PQR 1-   GTaw-6mm thick 
                        *PQR 2-   Smaw- 15 mm thick

What would be the thickness renge for base and weld metal?

for combined WPS,  base metal thickness range shall be 1.5mm to 30mm, am i correct?

Regards
Manpreet Singh


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...