Rinshu,

ERNiCrMo-3 weld metal is 100% Austentie, so there is no surprise that you get 0% ferrite.

I dont see any negative side of having no ferrite, you only need to take care having a clean surface free from any contamination, a contaminated surface would introduce P & S in the weld metal and can lead to microfissuring.

Your requirement for ferrite comes only in austenitic stainless steel weld metal which has 4 - 8% ferrite after solidification to swallow all those tramp elements.

Regards,

Praveen


--- On Thu, 12/30/10, rinshu <rinshad043@gmail.com> wrote:

> From: rinshu <rinshad043@gmail.com>
> Subject: [MW:9001] ER Ni Cr Mo-3 WELD OVERLAY
> To: "Materials & Welding" <materials-welding@googlegroups.com>
> Date: Thursday, December 30, 2010, 12:15 AM
> Dear all
>
> we have done CRO on SA516 Gr.70 ,we got ferrite content
> above 2.5mm
> from the weld interface as 0% will it have any negative
> effect on our
> CRO(ER NiCrMo-3-filler,SAW-process)
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members
> personel views and meant for educational purposes only,
> Users must take their own decisions w.r.t. applicable
> code/standard/contract documents.
>


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...