may be useful for the group members.
With best regards,
Prasad Joshi
> ----- Forwarded by Prasad Joshi/TPGAUH on 01/07/09 10:39 AM -----
> Dear Makarand
>
> Coming to your query, as per ASME B31.3 ASTM A 333/6 can be used below
> -45.5-deg. C (-50-deg. F as allowed by code without any special
> precautions) with following precautions:
>
> 1) Testing of Base metal at minimum design temperature (-60 deg C in your
> case.) as per B-3 of table 323.2.2 of B31.3. This is useful for the
> procurement part.
> 2) For fabrication and welding part, special precaution has to be
> specified
> for impact testing of Weld metal and HAZ. This is useful for specifying in
> the welding specification or construction specification. You will have to
> specially mention this in the p.class so that it will be highlighted to
> QA/QC or welding engineer.
>
> I hope this clarifies. Let me know if you need any further information.
>
> With best regards,
>
>
>
>
>
> Prasad Joshi
>
>
> PIPING
>
>
>
>
>
>
> Dear Prasad,
> I need your help. Can we use Material A333 Gr.6 for temp. Bellow -46
> deg.C.
> If yes then what backup document I should refer to prove it. I remember we
> have used this material upto -60 Deg. C, but I don't have any backup
> document to prove it. . if you have anything can you forward me.
> -Makarand.
>
>
>
> Save a tree...please don't print this e-mail unless you really need to.
>
>
>
>
>
>
>
>
>
> Save a tree...please don't print this e-mail unless you really need to.
>
>
> This email and any attached files ("Message") may contain confidential
> and/or privileged information. It is intended solely for the addressee(s).
> If you receive this Message in error, inform the sender by reply email,
> delete the Message and destroy any printed copy.
> Any unauthorized use, distribution, or copying of this Message or any part
> thereof is prohibited. Emails are susceptible to alteration. Neither
> Technip nor any of its affiliates shall be liable for the Message if
> altered or falsified nor shall they be liable for any damage caused by any
> virus that might be transmitted with this Message.
>
>
--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---
Comments