Re: [MW:35540] RANGE ASME SEC IX

  Dear Mr. Elavarasan,
  Plate to Pipe Qualification: A welder qualified on a plate is qualified to weld on pipe, but there are diameter and position restrictions
  Pipes of OD 24 and 26 inches, are well above 73 mm, so diameter is not a restricting factor for your case.
  For your 25 mm plate: The qual. range is 12.5 to 50 mm for production welds (with impact testing).
  24-inch pipe (9.5 mm wall):    Not qualified, as the wall thickness is less than the minimum qualified thickness of 12.5 mm.
  26-inch pipe (14 mm wall) :    Qualified, as the wall thickness is within the qualified range.
  8 mm wall thickness pipe:       Not qualified, as it is below the minimum qualified thickness.
  Welder Qualification (WQT): The same thickness rules apply to the welder as to the procedure, unless the welder was qualified
                                                   on pipe directly, in which case the thickness and diameter ranges may differ.
                                                                                  If you need to weld pipes with wall thickness less than 12.5 mm (such as 8 mm or 9.5 mm), you must                   
                                                   requalify the procedure and welder for that thickness range.
  Conclusion:
  • You cannot use the current plate WPS and WQT to weld a 24-inch pipe with 9.5 mm wall thickness or any pipe with 8 mm wall thickness.

  • You can use them for a 26-inch pipe with 14 mm wall thickness.

  • To weld thinner pipes (8 mm, 9.5 mm), you must qualify a new WPS and WQT for those thicknesses.

   Both 9.5 mm and 14 mm pipes generally require impact testing (as per ASTM A333/A333M-15 and other standards, especially    

   if impact properties are specified in the material grade or project specifications specify impact toughness as a mandatory property. 


   References:

   ASME Section IX, Table QW-451.1 and QW-452 

   Welder qualification diameter and thickness ranges.                                                                                                                                                                                                                                  

                                                                                                                                                                                                                                                                                                                                                                                                         Hope it is clear. 

   rgds,

   C Sridhar.

   -------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------


 


   





On Wed, 16 Apr 2025 at 12:27, Elavarasan Mech <elavarasan1861994@gmail.com> wrote:
Dear All

we have qualified WPS for ( ASME SEC IX)
1. BASE plate 8 mm ( 8TO 16 mm RANGE WITH IMPACT ) 
2 . BASE plate 25 mm ( 16TO 50mm RANGE WITH IMPACT ) 

Qualified WQT BASE PLATE THICKNESS :25 mm 
( 50 mm max ) 
My question is   Can we use this plate WPS and WQT  to weld 24inch pipe (9.5mm wall thickness )and 26 pipe(14mm wall thickness ) ,Welder can weld 8 mm wall thickness pipe ?                                  he qualified in 25 mm plate only  .please quide me

Regard 
ELAVARASAN


 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJ9L4ymSZ4aGa3XqiJswKMyr0sqCGWJO6xfGf_NCpqTSNFN5-A%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYiiyL0rY6PzhtTQCT2u-HKR_vXqisFY3JyQNuSRVnZwL2A%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...