Re: [MW:35539] RANGE ASME SEC IX

For WPS/PQR qualification, Diameter is an non essential variable according to ASME Sec.IX and position is a supplementary essential variable and only progression UP or DOWN counts.

For Welder Qualification check QW-461.9 Table & Table QW-452.3

Thanks & Regards

J.Gerald Jayakumar

0091-8838619635



On Wednesday 16 April, 2025 at 01:47:36 pm IST, Rilley Chellah Mulenga <rilley.mulenga@ahkgroup.com> wrote:


What is the diameter of the pipe to be welded , ASME IX give a limit on the diameter to be welded by a welder that has been qualified in a plate and what positions they can weld 

On Wed, 16 Apr 2025 at 08:57, Elavarasan Mech <elavarasan1861994@gmail.com> wrote:
Dear All

we have qualified WPS for ( ASME SEC IX)
1. BASE plate 8 mm ( 8TO 16 mm RANGE WITH IMPACT ) 
2 . BASE plate 25 mm ( 16TO 50mm RANGE WITH IMPACT ) 

Qualified WQT BASE PLATE THICKNESS :25 mm 
( 50 mm max ) 
My question is   Can we use this plate WPS and WQT  to weld 24inch pipe (9.5mm wall thickness )and 26 pipe(14mm wall thickness ) ,Welder can weld 8 mm wall thickness pipe ?                                  he qualified in 25 mm plate only  .please quide me

Regard 
ELAVARASAN


 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJ9L4ymSZ4aGa3XqiJswKMyr0sqCGWJO6xfGf_NCpqTSNFN5-A%40mail.gmail.com.


--
Thanks & kind regards


EmailLogo      

www.ahkgroup.com     

    
     Rilley Chellah Mulenga
     HEAD - MATERIALS EVALUATION

     T: +260 212 226431
     M:+26076123880/ 0964084833
     E:Rilley.Mulenga@ahkgroup.com


DISCLAIMER: The information in this Internet e-mail is confidential and may be legally privileged. It is intended solely for the addressee(s).
Access to this Internet e-mail by anyone else is unauthorised.

If you are not the intended recipient, any disclosure, copying, distribution or any action taken or omitted to be taken in reliance on it, is prohibited and may be unlawful.
All results and data contained in this document are subject to our Standard Terms and Conditions and are valid only when supported by an original document.

Please visit our website at www.ahkgroup.com

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHkXHT_qMzt7TESHXC2-%3DM3_7gmsbCznt5h4MhkxwYu7-GzNtg%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...