Re: [MW:33721] Bruscato X factor


X-factor is a calculation, or formula, that measures a weldment's resistance to temper embrittlement, a brittleness or loss of toughness that occurs when the weldment is held (or slowly cooled) through a temperature range of approximately 850 to 1,100 degrees F.04-May-2010

On Thu, 17 Nov 2022 at 10:02, Prakash Hegde
<pb.hegde@yahoo.com> wrote:

Bruscato X factor (2).

J=(Mn + Si)(P + Sn) x104 (in wt %), has been applied to parent steels and 

weld metals.

X=(10P + 5Sb + 4Sn + As)/100 (in ppm), is applied to weld metals.



On Thu, 17 Nov 2022 at 8:47, Vishwas Keskar
<vvkeskar123@gmail.com> wrote:
Refer API 934 A 
You can details 


Sent from my iPhone

On 16-Nov-2022, at 8:59 AM, Pravin Poornachandran <htcispravin@gmail.com> wrote:

Dear Expert,

Can anyone share or explain how to calculate Bruscato X factor for Gr.22 grade especially on welding consumable chemical composition.

Mind sharing any supporting document or article on how to calculate X factor. 

In my knowledge, X factor is trace elements which usually not guaranteed by manufacturer and it's unintentionally added such as Sn, Sb, As etc.

Best regards,
Pravin 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADDyn7eDnamAySywpAepJJvDTzjvqr3C7bOJ1OQGP9cr3S5zug%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/47B7DCC9-38CF-455D-B1B9-DA4F05AF6191%40gmail.com
.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/539548265.1097481.1668659654176%40mail.yahoo.com.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...