Tuesday, November 15, 2022

Re: [MW:33712] 410 WPS PQR

if BM carbon <= 0.08% .. u can do it without PWHT .. E309L-16 .. preheat 300c and interpass < 300C 
else PWHT is essential for avoiding cracks 
U can go for 410S if possible

Best Regards ,
Ahmed Osman

On Tuesday, November 15, 2022 at 11:51:39 a.m. GMT+3, Vishwas Keskar Welding Manager WELDING <vvkeskar123@gmail.com> wrote:


Experts,

Pl. guide for qualifying PQR for SA 240 TYP 410 without PWHT .
Pl, guide for Pre heating, inter pass  temperature, consumable to be used 
Thickness of job is 8 mm , 10mm

Thanks and regards
Vishwas - IWE
International Welding Engineer 
Head - Welding Technology

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/8369c986-7b85-44d3-b06c-2670d887ee26n%40googlegroups.com.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...