Hi,
Since this is P.No.1,Low temperature material, why do you go for ER80S-Ni1 ? Its used for weathering steel and corrosion resistant applications. It can be used to weld SA350, LF5 (P.No.9A) which is 1.5Ni steel

SA350, LF2 and SA333 Gr.6 are C-Mn-Si steel (P.No.1), for this ER70S2 or ER70S-6 are fine. Electrode E7018-1

Thanks& Regards,

 

(Karthik)

Karthikeyan.S

M: +66-892512282

E-mail : karthik6684@yahoo.com



On Tuesday, June 30, 2020, 04:09:54 PM GMT+7, K K <karan.hbl@gmail.com> wrote:


Thanks for your response.

Please explain to me why I can't use ER80S-Ni1 for AWS 5.28 GTAW process according to the table - A1 API 582. 


Thanks 

Kiran

On Tuesday, June 30, 2020 at 9:11:14 AM UTC+5:30, Karthik wrote:
Hi,
You can use E7018-1 / ER70S-1B / ER70S-6

Inline image


Thanks& Regards,

 

(Karthik)

Karthikeyan.S

M: +66-892512282

E-mail : karthi...@yahoo.com



On Monday, June 29, 2020, 09:51:39 PM GMT+7, K K <kara...@gmail.com> wrote:


Dear Experts.

Can anyone suggest to according to API 582 as per TABLE - A1 has not recommended ER80S-Ni1 for AWS 5.28 GTAW process.

Please explain to me in detail the table - A1 API 582 and which electrode shall I use for the below-mentioned material.

PQR material - ASTM A333 Gr.6 to ASTM A350 LF2.

PQR Thickness - 12.7 mm.

Impact tested - -46°C

Thanks and regards,

Kiran

--
https://materials-welding. blogspot.com/
https://www.linkedin.com/ groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@ googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/ msgid/materials-welding/ dbf583fe-f42a-4eb3-9975- 5c62126d6ef2o%40googlegroups. com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/51e46130-64fa-498d-8fda-2d911143609eo%40googlegroups.com
.

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...