RE: [MW:31054] 3 Cycle PWHT requirements acc.to ASME

There is no requirement within ASME Section I or Section VIII to perform a simulated PWHT for three cycles.  This a common requirement in petro-chemical specifications and, occasionally, other customer specifications.

 

See Section VIII, Division 1, UCS-85, "Heat Treatment of Test Specimens" for base metal simulated heat treatment requirements.  This is typically a single cycle mimicking the production heat treatment.

 

There is no comparable requirement in ASME Section I.

 

Hope this helps.  Code is fun.

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of José Juan Jiménez Alejandro
Sent: Saturday, June 27, 2020 12:26 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:31046] 3 Cycle PWHT requirements acc.to ASME

 

I have never seen in the ASME Code (Section I and VIII Div. 1) that mentions anything about three cycles of a PWHT, the PWHT tables in these two ASME sections are very clear in terms of materials, times and temperatures.

Regards!.

 

El vie., 26 jun. 2020 a las 22:08, 'james gerald' via Materials & Welding (<materials-welding@googlegroups.com>) escribió:

Please provide the ASME Code reference where the 3 cycle PWHT is specified to understand your exact requirement.

 

Thanks & Regards

J.Gerald Jayakumar

 

 

On Friday, June 26, 2020, 10:35:50 PM GMT+7, Kiran Ekbote <karan.hbl@gmail.com> wrote:

 

 

Sir, 

 

  Thanks for your reply,   


Heat Treatment required for the Weld.

can you describe more on this topic, regarding Mechanical test and hardness test?

What is the time required for one cycle and for 3 cycles?

 

 

On Fri, Jun 26, 2020 at 2:23 PM 'james gerald' via Materials & Welding <materials-welding@googlegroups.com> wrote:

Is the Heat Treatment required for Plates or for the Welds.

 

If it is for the Plates during the procurement stage, then you need to follow the same Heat Treatment simulating the exact condition it undergoes.

 

1. Initial Heat Treatment for the Plates will be the first cycle.

2. PWHT after welding will be the second cycle

3. Taking into account the Repair after PWHT will be the 3rd cycle.

 

You can simulate the same condition on one coupon and undergo the test as per Material standard.

 

If it is for Welds, then you can apply PWHT in one cycle as the snap short  below.

 

One Coupon and the testing requirements as per ASME Sec.IX and applicable specifications.

 

Thanks & Regards

J.Gerald Jayakumar

 

 

On Friday, June 26, 2020, 12:12:39 PM GMT+7, K K <karan.hbl@gmail.com> wrote:

 

 

Dear All,

 

Expertise can you please see my query, Can I get the solution to the below query.

 

How to Calculate 3 cycle PWHT, What are the requirements? please explain to me in detail.

 

What are the initial requirements and what are mechanical and hardness requirements? 

 

Please explain to me in detail with a step vise.

 

I hope i will get a good response from the Materials & Welding team and from Expertise.

 

Thanks

 

Kiran


On Wednesday, June 24, 2020 at 12:10:59 PM UTC+5:30, K K wrote:

Thanks for your support.

 

 

Regarding PWHT of 3 cycles.

 

Below I have mentioned my PQR ranges for PWHT.

 

POST WELD HEAT TREATMENT( QW-407)

TEMPERATURE RANGE 630 ±10° C

SOAKING PERIOD 190Min

HEATING RATE 190°C/Hours Max

COOLING RATE 190°C/Hours Max.

As per the above range, it's qualified 3 cycles, but how? and for 3 Cycles PWHT where I required test coupons? how many coupons tests shall I have conduct?

Please clarify my above query in detail with code.

 

Thanks once again.

 

Kiran

 


On Tuesday, June 23, 2020 at 11:43:19 AM UTC+5:30, petervsoloman wrote:

Dear Kiran,

Once PWHT competed for joints due to modification cut/reweld or repair re PWHT required that particular joints.

it is mention in the procedure is enough to do the job. This you can mention in your weld repair procedure.

Regards,

PETER SOLOMAN

+971 33663119

 

On Mon, Jun 22, 2020 at 7:32 AM K K <kara...@gmail.com> wrote:

Dear All,

 

Please describe to me regarding 3 cycle PWHT requirements as per ASME.

 

If my PQR tested with two coupons where I required one more test coupon and additional one more for repair.

 

Please explain to me in detail and related to mechanical testing for PWHT.

 

What is the meaning of this paragraph - **an additional one PWHT cycle shall be incorporated to simulate field repair or modification.**

 

Thanks and Regards

Kiran

--
https://materials-welding. blogspot.com/
https://www.linkedin.com/ groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/ msgid/materials-welding/ 2b255cdf-b673-4981-8fcf- ad1fb4863ecbo%40googlegroups. com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit

https://groups.google.com/d/msgid/materials-welding/88e3f572-9b04-4790-bdbc-cca1667fc306o%40googlegroups.com

.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1700708950.2832782.1593157682597%40mail.yahoo.com.


 

--


KIRAN

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMFjUk7zY2e8yd784D1i57j3WFLVoXxf_wHR4i1fPeTsWJLC5A%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/299870276.3117366.1593218167469%40mail.yahoo.com.


 

--

Ing. José Juan Jiménez Alejandro

Independent Consultant in Parts

and Pressure Equipment

SSI-TPI

Móvil +52 1 812 352 4606

Skype: jjjimeneza

 

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAO5Zur%2B3wN6%3Dab77bXffxpPis%2BoAWpbG46RuT-SoaKkm82zo6g%40mail.gmail.com.

DISCLAIMER This e-mail and any attachments thereto may contain information which is confidential and/or protected by intellectual property rights and are intended for the sole use of the recipient(s)named above. Any use of the information contained herein (including, but not limited to, total or partial reproduction, communication or distribution in any form) by persons other than the designated recipient(s) is prohibited. If you have received this e-mail in error, please notify the sender either by telephone or by e-mail and delete the material from any computer.
General Data Protection Regulation (GDPR)
We respect and protect your privacy to provide you with our services. Please read https://www.hamon.com/customer-data-protection-notice (Customer) and https://www.hamon.com/seller-data-protection-notice (Supplier) how we process your personal data.

Thank you for your cooperation.
______________________________________________________________________

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...