We're it is given we can change backing .only removal is given.
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Friday, August 31, 2018
[MW:28239] Combination of welding process on wos
if two welders qualify for combination of diff welding process on separate test coupon than both welder can make welding on same joint during production?
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Re: [MW:28239] water sample parameters for hydro test
It has to be a non-flammable liquid, and also non-lethal, some customers ask in their specification that the water is free of salts and minerals, that you show by a documented laboratory test, but in general I would recommend that you review UG-99 of Section VIII DIV.1 of the BPVC ASME, in case this is your Construction Code.
Regards! .
El vie., 31 ago. 2018 a las 8:03, Temburu Chiranjeevulu (<chiru.qaqc@gmail.com>) escribió:
--Dear Experts,What are the parameters of water sample, we have to check before hydro static test.Thanks and Best Regards,CHIRANJEEVULU T,8790956353.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Ing. José Juan Jiménez Alejandro
ASME Independent Consultant
and Technical Manager SSI-TPI
Cel. +52 812 352 4606
Skype: jjjimeneza
Twitter: @jjjimeneza
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
[MW:28238] water sample parameters for hydro test
Dear Experts,
What are the parameters of water sample, we have to check before hydro static test.
Thanks and Best Regards,
CHIRANJEEVULU T,
8790956353.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Wednesday, August 29, 2018
Re: [MW:28237] Tensile properties of 6010 and API 5L X70 Pipe
you can go ahead considering the hardness test .
On Thu, Aug 9, 2018 at 5:18 PM 'Asif Shahzad' via Materials & Welding <materials-welding@googlegroups.com> wrote:
--Dear Expert,we need to weld the API 5L X70 grade pipe and using the electrode 6010 for root, While tensile strength of the 6010 electrode is 430 MPa while tensile strength of X70 grade is (570 to 760)MPa. So tensile strength of 6010 is lower than x70.For hot pass, filling and capping we are using 9010.Please provide your expert opinion that we can use the electrode having low tensile strength than the base metal and if yes kindly give the reasonRegards,Asif
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Regards,
Styendra Kumar Tripathi
Mo. No. +919650805549
Styendra Kumar Tripathi
Mo. No. +919650805549
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
[MW:28236] VERTICAL SEAM CLADDING
Dear Experts,
-- I would like to know details of Vertical Seam Cladding on Tanks. We carried out cladding previously which was conventional method but this method we have not done.
Would like to know what is the method to carry out and how the sheets to be fabricated.
Thanks in advance.
Regards,
Vijay
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Re: [MW:28235] criteria for ASTM G 28
Hi All.
I have found recently total specification of "GS EP PVV 618" that say 3mm/year(ideally 1-1.2mm/year) for acceptance of G28.
Now does any body know why this amount specified in spite of other documents (that mentioned .8 or .9 mm/year ) and when ideally amount applicable for setting criteria?
Regards.
On Wed, Jul 25, 2018 at 10:10 AM <nithindsilva4u@gmail.com> wrote:
Hi pls find my reply,--1. Same criteria will apply to weld and materials.We have done this test for weld as well as parent materials (Mill as well as in shop Lab) successfully and could achieve corrosion rates less than 0.8mm/year.Sent from my iPhoneDear Joseph.Thank you so much. I have found a reference in mentioned address web mail which have been attached.Based on this image, the acceptance criteria for 625 is 0.9 but there is two item that weaken applicability of it, at title of table said unwelded and in second column that highlighted to as-received.1.what is your idea, this criteria can be used for weld and clad or not?2.and in title of G28 applicable for wrought Ni alloys, nevertheless is it applicable for weld qualification?Regards.--On Tue, Jul 24, 2018 at 2:09 PM, Nithin Joseph <nithindsilva4u@gmail.com> wrote:Hi,It depends on client, I have gone through the specs of end users such as ADCO, Tatweer, PDO and they clearly state that it should not exceed 0.9mm/year.You can also visit below article to know the widely followed corrosion rates for various alloys with their corrosion rates.--On Tue, Jul 24, 2018 at 10:58 AM, Ali Asghari <asgharialigl@gmail.com> wrote:Hi.Thanks.Would you send documents that mentioned this criteria,unfortunately in our documents only referee to G28.Thanks.On Tue, Jul 24, 2018 at 9:51 AM, Nithin Joseph <nithindsilva4u@gmail.com> wrote:Hi,You should check client spec and most of the standards give the requirements as 0.9mm/year.On Mon, Jul 23, 2018 at 9:07 AM, Ali Asghari <asgharialigl@gmail.com> wrote:Dear Shyamal.unfortunately in my project specification referred to ASTM G28.Do you have any access to reference documents that addressed in the document?and would you say in your project spec how much specify to corrosion rate of G28?Regards
On Sunday, July 22, 2018 at 9:07:51 AM UTC+4:30, shyamal das wrote:Hi,Acceptance criteria depends upon the project specificationsKrShyamalOn 10 July 2018 at 17:15, Ali Asghari <asghar...@gmail.com> wrote:Dear All.--Does anybody have any documents that said about criteria for ASTM G28 OF INCONEL CLAD?Regards
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
--Regards,
Nithin Joseph Dsilva+971 557645785You received this message because you are subscribed to a topic in the Google Groups "Materials & Welding" group.
To unsubscribe from this topic, visit https://groups.google.com/d/topic/materials-welding/2U8FTJdMvvA/unsubscribe.
To unsubscribe from this group and all its topics, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
--Regards,
Nithin Joseph Dsilva+971 557645785
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to a topic in the Google Groups "Materials & Welding" group.
To unsubscribe from this topic, visit https://groups.google.com/d/topic/materials-welding/2U8FTJdMvvA/unsubscribe.
To unsubscribe from this group and all its topics, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
<20180724_173051_001.jpg>
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to a topic in the Google Groups "Materials & Welding" group.
To unsubscribe from this topic, visit https://groups.google.com/d/topic/materials-welding/2U8FTJdMvvA/unsubscribe.
To unsubscribe from this group and all its topics, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Re: [MW:28233] sample preparation of ASTM G28
Hi,
The sample preparation for clad materials is always debatable and should mostly be addressed by end user specification. It should be dictated from the fact that service fluid is in touch with the final clad layer and considering the corrosion allowance. However you may check the entire cross section corrosion rates for your reference.
Thanks & Regards,
Harish
Harish
On Aug 29, 2018 12:10 PM, "Ali Asghari" <asgharialigl@gmail.com> wrote:
Dear All.Does anybody have any experiences or instruction for preparation of sample for G28?is there any requirement to remove clad material from surface and go through it or not?this question arises from this point that IGC comes from carbide & inter metallics that mostly possible in diluted area and also accepted corrosion rate is about 0.9 mm/year for 625. Now is it reasonable to prepare sample from interface or without removing of thickness and take it from surface?Regards.--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Re: [MW:28234] sample preparation of ASTM G28
Dear Harish.
Thank you for responding.
"The intent is to test a specimen representing as nearly as possible the material as used in service. The specimens should be cut to represent the grain flow direction that will see service, for example, specimens should not contain cross-sectional areas unless it is the intent of the test to evaluate these. Only such surface finishing should be performed as is required to remove foreign material and obtain a standard, uniform finish as specified in 6.4. For very heavy sections, specimens should be maintained to represent the appropriate surface while maintaining reasonable specimen size for convenience in testing. Ordinarily, removal of more material than necessary will have little influence on the test results." this paragraph is taken from G28 and only said about the surface area but didn't talk about any thing about cross section or through thickness orientation of sample especially for weld deposited over laid that have a metallurgical & diluted interface can rise possibility of detrimental phase.
Do you have any experience or document that address this issue?
Regards.
On Wed, Aug 29, 2018 at 11:27 AM Harish Kannepalli <harishkannepalli@gmail.com> wrote:
Hi,The sample preparation for clad materials is always debatable and should mostly be addressed by end user specification. It should be dictated from the fact that service fluid is in touch with the final clad layer and considering the corrosion allowance. However you may check the entire cross section corrosion rates for your reference.Thanks & Regards,
Harish--On Aug 29, 2018 12:10 PM, "Ali Asghari" <asgharialigl@gmail.com> wrote:Dear All.Does anybody have any experiences or instruction for preparation of sample for G28?is there any requirement to remove clad material from surface and go through it or not?this question arises from this point that IGC comes from carbide & inter metallics that mostly possible in diluted area and also accepted corrosion rate is about 0.9 mm/year for 625. Now is it reasonable to prepare sample from interface or without removing of thickness and take it from surface?Regards.--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to a topic in the Google Groups "Materials & Welding" group.
To unsubscribe from this topic, visit https://groups.google.com/d/topic/materials-welding/lBI4bYhNtZQ/unsubscribe.
To unsubscribe from this group and all its topics, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
[MW:28232] sample preparation of ASTM G28
Dear All.
-- Does anybody have any experiences or instruction for preparation of sample for G28?is there any requirement to remove clad material from surface and go through it or not?
this question arises from this point that IGC comes from carbide & inter metallics that mostly possible in diluted area and also accepted corrosion rate is about 0.9 mm/year for 625. Now is it reasonable to prepare sample from interface or without removing of thickness and take it from surface?
Regards.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Monday, August 27, 2018
Re: [MW:28231] HEAT INPUT Vs IMPACT
Hi,
Please find attached a document on key concept regarding heat input and impact value, submitted earlier. It should clear some basic doubts.
Best Regards,
Shashank C Vagal (Quality Adviser), (+91) 8082395502, 8779046302,
NEO METAL-ANALYST & NDT SERVICES
· A-25, Geet Siddhi, Boradevadi, Moshi-Haveli, PCMC, Pune 412105
· 301, PRATHAMESH, M G Rd – Mahant Rd, Vile Parle East, Mumbai 400 057 INDIA
www.neometalanalystndt.com / enquiry@neometalanalystndt.com / nach_sam@yahoo.com
On Monday, 27 August, 2018, 3:29:54 PM IST, Aslam Khan <aslamkhan15@gmail.com> wrote:
Heat Input(J/mm) = (Amperage x Voltage x 60)/Travel Speed
Please check QW-409.1 for detail description..
On Mon 27 Aug, 2018, 8:10 AM Kannayeram Gnanapandithan, <kgpandithan@gmail.com> wrote:
What is the formula for calculating Heat input. Interpass temp is also important to achieve good impact values--On Mon, 27 Aug 2018 8:06 am Paresh Katvi, <pkatvi@gmail.com> wrote:Not only travel speed but also selection of the welding consumables.Regards,Paresh--On Sun, 26 Aug 2018, 15:31 CHITTARANJAN BHIWANDKAR, <crbhiwandkar.smspl@gmail.com> wrote:Thanks PARESH,In other words the Impact values in MTCcan be a governing value to decide on travel speed.--On Sun, 26 Aug 2018, 12:36 p.m. Paresh Katvi, <pkatvi@gmail.com> wrote:HiIn my opinion, Heat input is a crucial criteria to achieve impact values in Weld, HAZ and Parent Metal. Travel speed is one of important contributor for determining heat input. Again it is very important , which material , thickness and welding process used for establishing heat input to achieve desired toughness property.You need to referred your historical records in order to judge and establish heat input parameters to achieve particular range of impact values in given material.Regards,Paresh--On Thu, Aug 23, 2018 at 4:35 PM BHIWANDKAR C R <crbhiwandkar.smspl@gmail.com> wrote:SIR,--WHILE PREPARING WPS THE CONSIDERATION OFHEAT INPUT JOULES TO JOULES ON MILL T CIS REQUIRED TO BE DONE. OR THE TRAVEL SPEEDCAN BE DETERMIND ON THE BASIS OF THE IMAPACTTEST VALUES GIVEN ON MILL TC
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Re: [MW:28230] HEAT INPUT Vs IMPACT
Heat Input(J/mm) = (Amperage x Voltage x 60)/Travel Speed
Please check QW-409.1 for detail description..
On Mon 27 Aug, 2018, 8:10 AM Kannayeram Gnanapandithan, <kgpandithan@gmail.com> wrote:
What is the formula for calculating Heat input. Interpass temp is also important to achieve good impact values--On Mon, 27 Aug 2018 8:06 am Paresh Katvi, <pkatvi@gmail.com> wrote:Not only travel speed but also selection of the welding consumables.Regards,Paresh--On Sun, 26 Aug 2018, 15:31 CHITTARANJAN BHIWANDKAR, <crbhiwandkar.smspl@gmail.com> wrote:Thanks PARESH,In other words the Impact values in MTCcan be a governing value to decide on travel speed.--On Sun, 26 Aug 2018, 12:36 p.m. Paresh Katvi, <pkatvi@gmail.com> wrote:HiIn my opinion, Heat input is a crucial criteria to achieve impact values in Weld, HAZ and Parent Metal. Travel speed is one of important contributor for determining heat input. Again it is very important , which material , thickness and welding process used for establishing heat input to achieve desired toughness property.You need to referred your historical records in order to judge and establish heat input parameters to achieve particular range of impact values in given material.Regards,Paresh--On Thu, Aug 23, 2018 at 4:35 PM BHIWANDKAR C R <crbhiwandkar.smspl@gmail.com> wrote:SIR,--WHILE PREPARING WPS THE CONSIDERATION OFHEAT INPUT JOULES TO JOULES ON MILL T CIS REQUIRED TO BE DONE. OR THE TRAVEL SPEEDCAN BE DETERMIND ON THE BASIS OF THE IMAPACTTEST VALUES GIVEN ON MILL TC
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
[MW:28229] SSC of Martensite stainless steel
Dear All.
-- Does anybody have datailed procedure for SSC testing of CRA especially for martensite stainless steel except as EFC17 ?
Regards.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Re: [MW:28228] HEAT INPUT Vs IMPACT
What is the formula for calculating Heat input. Interpass temp is also important to achieve good impact values
On Mon, 27 Aug 2018 8:06 am Paresh Katvi, <pkatvi@gmail.com> wrote:
Not only travel speed but also selection of the welding consumables.Regards,Paresh--On Sun, 26 Aug 2018, 15:31 CHITTARANJAN BHIWANDKAR, <crbhiwandkar.smspl@gmail.com> wrote:Thanks PARESH,In other words the Impact values in MTCcan be a governing value to decide on travel speed.--On Sun, 26 Aug 2018, 12:36 p.m. Paresh Katvi, <pkatvi@gmail.com> wrote:HiIn my opinion, Heat input is a crucial criteria to achieve impact values in Weld, HAZ and Parent Metal. Travel speed is one of important contributor for determining heat input. Again it is very important , which material , thickness and welding process used for establishing heat input to achieve desired toughness property.You need to referred your historical records in order to judge and establish heat input parameters to achieve particular range of impact values in given material.Regards,Paresh--On Thu, Aug 23, 2018 at 4:35 PM BHIWANDKAR C R <crbhiwandkar.smspl@gmail.com> wrote:SIR,--WHILE PREPARING WPS THE CONSIDERATION OFHEAT INPUT JOULES TO JOULES ON MILL T CIS REQUIRED TO BE DONE. OR THE TRAVEL SPEEDCAN BE DETERMIND ON THE BASIS OF THE IMAPACTTEST VALUES GIVEN ON MILL TC
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Re: [MW:28227] HEAT INPUT Vs IMPACT
Not only travel speed but also selection of the welding consumables.
Regards,
Paresh
On Sun, 26 Aug 2018, 15:31 CHITTARANJAN BHIWANDKAR, <crbhiwandkar.smspl@gmail.com> wrote:
Thanks PARESH,In other words the Impact values in MTCcan be a governing value to decide on travel speed.--On Sun, 26 Aug 2018, 12:36 p.m. Paresh Katvi, <pkatvi@gmail.com> wrote:HiIn my opinion, Heat input is a crucial criteria to achieve impact values in Weld, HAZ and Parent Metal. Travel speed is one of important contributor for determining heat input. Again it is very important , which material , thickness and welding process used for establishing heat input to achieve desired toughness property.You need to referred your historical records in order to judge and establish heat input parameters to achieve particular range of impact values in given material.Regards,Paresh--On Thu, Aug 23, 2018 at 4:35 PM BHIWANDKAR C R <crbhiwandkar.smspl@gmail.com> wrote:SIR,--WHILE PREPARING WPS THE CONSIDERATION OFHEAT INPUT JOULES TO JOULES ON MILL T CIS REQUIRED TO BE DONE. OR THE TRAVEL SPEEDCAN BE DETERMIND ON THE BASIS OF THE IMAPACTTEST VALUES GIVEN ON MILL TC
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Sunday, August 26, 2018
Re: [MW:28226] Re: Tensile properties of 6010 and API 5L X70 Pipe
PLS SPECIFY DIA.& THK. OF THE PIPE
Thanks/Regards,
C.R.Bhiwandkar
Supreme Megastructures Pvt. Ltd.
Supreme House, Plot No.-49/C,
Pratap Gad, Opp.-IIT Main Gate.
Powai, Mumbai - 400076
Cell No.:-+919867139337
On Sun, Aug 26, 2018 at 4:36 PM Mohd Siraj <mohd52100@gmail.com> wrote:
--asif,6010+9010 (or 9018 up hill)would be good choice,8010 would may lead to hot cracking...
On Thursday, August 9, 2018 at 2:48:37 PM UTC+3, Asif Shahzad wrote:Dear Expert,we need to weld the API 5L X70 grade pipe and using the electrode 6010 for root, While tensile strength of the 6010 electrode is 430 MPa while tensile strength of X70 grade is (570 to 760)MPa. So tensile strength of 6010 is lower than x70.For hot pass, filling and capping we are using 9010.Please provide your expert opinion that we can use the electrode having low tensile strength than the base metal and if yes kindly give the reasonRegards,Asif
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
[MW:28225] Re: Tensile properties of 6010 and API 5L X70 Pipe
asif,
6010+9010 (or 9018 up hill)would be good choice,
8010 would may lead to hot cracking...
On Thursday, August 9, 2018 at 2:48:37 PM UTC+3, Asif Shahzad wrote:
Dear Expert,we need to weld the API 5L X70 grade pipe and using the electrode 6010 for root, While tensile strength of the 6010 electrode is 430 MPa while tensile strength of X70 grade is (570 to 760)MPa. So tensile strength of 6010 is lower than x70.For hot pass, filling and capping we are using 9010.Please provide your expert opinion that we can use the electrode having low tensile strength than the base metal and if yes kindly give the reasonRegards,Asif
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Re: [MW:28224] HEAT INPUT Vs IMPACT
Thanks PARESH,
In other words the Impact values in MTC
can be a governing value to decide on travel speed.
On Sun, 26 Aug 2018, 12:36 p.m. Paresh Katvi, <pkatvi@gmail.com> wrote:
HiIn my opinion, Heat input is a crucial criteria to achieve impact values in Weld, HAZ and Parent Metal. Travel speed is one of important contributor for determining heat input. Again it is very important , which material , thickness and welding process used for establishing heat input to achieve desired toughness property.You need to referred your historical records in order to judge and establish heat input parameters to achieve particular range of impact values in given material.Regards,Paresh--On Thu, Aug 23, 2018 at 4:35 PM BHIWANDKAR C R <crbhiwandkar.smspl@gmail.com> wrote:SIR,--WHILE PREPARING WPS THE CONSIDERATION OFHEAT INPUT JOULES TO JOULES ON MILL T CIS REQUIRED TO BE DONE. OR THE TRAVEL SPEEDCAN BE DETERMIND ON THE BASIS OF THE IMAPACTTEST VALUES GIVEN ON MILL TC
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Re: [MW:28223] HEAT INPUT Vs IMPACT
Hi
In my opinion, Heat input is a crucial criteria to achieve impact values in Weld, HAZ and Parent Metal. Travel speed is one of important contributor for determining heat input. Again it is very important , which material , thickness and welding process used for establishing heat input to achieve desired toughness property.
You need to referred your historical records in order to judge and establish heat input parameters to achieve particular range of impact values in given material.
Regards,
Paresh
On Thu, Aug 23, 2018 at 4:35 PM BHIWANDKAR C R <crbhiwandkar.smspl@gmail.com> wrote:
SIR,--WHILE PREPARING WPS THE CONSIDERATION OFHEAT INPUT JOULES TO JOULES ON MILL T CIS REQUIRED TO BE DONE. OR THE TRAVEL SPEEDCAN BE DETERMIND ON THE BASIS OF THE IMAPACTTEST VALUES GIVEN ON MILL TC
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Re: [MW:28222] Throat Thickness in welding between DIN-18800 part 1 & EN1993 part 1
Check asme B 31.3 or 31.1 are incorporating with your requirements, if not there will be client specifications where his requirements ensured with the reference to international codes.
Regards
Muneeb.
On Sat, Aug 25, 2018, 1:04 PM 'Bijay' via Materials & Welding <materials-welding@googlegroups.com> wrote:
--Dear ExpertsIn one of my project I have facing problems in throat thickness of welding.Our governing code for welding is DIN - 18800 part 1, but as per clients instruction we have to follow the EN 1993 part 1 for throat thickness.I can't find anything regarding throat thickness. Please guide what to do ?Thank you in advance.With RegardsBijay Kumar ChoudhuryMob +91 8980630973
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Subscribe to:
Posts (Atom)
[MW:35668] Selection of Filler/Electrode.
Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...
-
Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? ...
-
Definition of buttering from ASME Section IX, QW/QB-492 Definitions: Buttering: the addition of material, by welding, on one or bot...
-
Section I. PRINT READING 3-1. GENERAL a. Drawings . Drawing or sketching is a universal language used to convey all necessary information to...