Re: [MW:26352] Hardfacing overlay on cast iron glassmould

try a buttering layer with nicr 80/20 powder

On Sat, Apr 1, 2017 at 3:36 PM, <arcraftplasma@gmail.com> wrote:


Hi Experts,

 

I am welding a PTA overlay of - Colmonoy 42-P2 Powder on a Cast iron glass mould. We are facing a problem of porosity. We have taken care of cleanliness, quality and quantity of shielding gas etc. Will be glad to read suggestions on eliminating the porosity.

 

Parameters are

Current 63 amps

Volts   24 V

Pre Heat Temp 450 C

 

Chemical composition of Cast Iron

 C            3.55        ± 0.10

Mn         0.6          ± 0.10

Si             2              ± 0.20

P             < 0.10    ± 0.20

S              < 0.10    ± 0.20

Cr            < 0.10    ± 0.20

Ni            < 0.10    ± 0.20

Mo         0.45        ± 0.05

V             0.13        ± 0.03

Ti             < 0.10    ± 0.03

Ceq.       4.15        ± 0.10

 

Chemical composition of Powder

Boron    1.64

Carbon 0.37

Cobalt   0.10

Chromium           10.00

Iron        2.48

Nickel    Balance

Silicon   3.07

 

Suggestions most welcome. Thanks in advance.

 

S. Vignesh

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/791f2eb6-0f74-4bfb-a901-34fa9516b4b3%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJPeGUnbpiSLUMQrSUhn7CUwrBNhAA48DMmEyRVHGEjw18NqRg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35289] Welding consumable for S355J2WP material

S355 J2 WP  is a weathering structural steel  It has better atmospheric corrosion resistance. Use E 8018 - W1/W2  Electrodes This is regular...