Friday, March 10, 2017

Re: [MW:26183] Can we use E 309L consumable for joining of A105vlave+ 316Ti pipe?

if we use 309, FN will be more and no chance for Hot cracking??

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Thu, Mar 9, 2017 at 10:52 PM, dilintas <dilintas@gmail.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (dilintas@gmail.com) Add cleanup rule | More info

To avoid low FN and thus hot cracking,  309 with low dilution rate  is a must



Sent from my Samsung Galaxy smartphone.

-------- Original message --------
From: 'Sankaran Sp' via Materials & Welding <materials-welding@googlegroups.com>
Date: 08/03/2017 13:07 (GMT+03:00)
To: Materials & Welding <materials-welding@googlegroups.com>
Subject: [MW:26160] Can we use E 309L consumable for joining of A105 vlave+ 316Ti pipe?

Dear friends,

Can you clarify the following points?

we are planning to welding of nipple(pipe) of A 269 TP 316Ti pipe with A105 forged steel valve, welding is socket weld( fillet ) only. while welding of these combination can we use Er 309L type consumable? or any Ti added consumable to be used? 
no specific requirement from customer, kindly clarify and do the needful.

Regards,

Sankaran.sp 
welding& metallurgy expert 
coimbatore, india.     

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/gkschhpxuiibm0rrb3l2uxw9.1489080121564%40email.android.com.
For more options, visit https://groups.google.com/d/optout.


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eNyMDqkcE6H3sHfZGeugT61Zi2CgD00em0-b7uKicvNiA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35289] Welding consumable for S355J2WP material

S355 J2 WP  is a weathering structural steel  It has better atmospheric corrosion resistance. Use E 8018 - W1/W2  Electrodes This is regular...