In that case first  PQR on 10mm plate without PWHT which will qualify from 1.5 mm to 20mm .

Second PQR on say 30mm with PWHT which will qualify from above 20 mm to 60 mm considering PWHT requirements for CS as per B 31.3.

And in WPS , in QW 407 section  need to mention that PWHT is applicable for only above 20mm.

Reference QW 200 .2  section f

Regards,

Anup

On 29 Apr 2015 07:01, "S.Mohammed" <mohd52100@gmail.com> wrote:
anup,

if design code is b31.3 then how could u combine with pwht and without pwht wps?

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/d3ff6c05-bc6b-487e-912b-0b616c5a9c1a%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJsQutYcWPYny8_YOJbaw9hvRm0QtBnciLwayjBMhd0U2jrPuw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...