Thursday, April 16, 2015

Re: [MW:23109] Normal duplex and super duplex

You weld needs to cool slower to give time for ferrite to develop. Could you send me the process parameters?

Sent from my BlackBerry 10 smartphone.
From: Pravin G
Sent: Τετάρτη, 15 Απριλίου 2015 - 17:18
To: materials-welding@googlegroups.com
Reply To: materials-welding@googlegroups.com
Subject: Re: [MW:23104] Normal duplex and super duplex

Dear Sir,

Our requirement for FN is 35-65, however we are getting exactly 35 which is border line for several test which is unacceptable by the client.

Kindly advice with your expertise.
Pravin Poornachandran


Sent from my iPhone

On 15 Apr 2015, at 15:22, george.dilintas@gr.bureauveritas.com wrote:

You are getting low or high ferrite?

best regards

Dr. Georgios Dilintas

Authorized Nuclear Inspector
Authorized Inspector Supervisor

I&F REGIONAL TECHNICAL MANAGER
BUREAU VERITAS PIRAEUS - GREECE

Tel: +30 210 40 63 113 /4 /5
Fax: +30 210 40 63 118
Cell: +30 69 44 64 62 04


<graycol.gif>Pravin G ---15/04/2015 06:29:23---Dear expert, I'm having to weld normal duplex plate for vessel, SMAW process with following requirem

From: Pravin G <htcispravin@gmail.com>
To: materials-welding@googlegroups.com
Date: 15/04/2015 06:29
Subject: [MW:23095] Normal duplex and super duplex
Sent by: materials-welding@googlegroups.com





Dear expert,

I'm having to weld normal duplex plate for vessel, SMAW process with following requirements:

I.v -40degC
FN: 35-65
CPT 22deg C @24 hrs
Corrosion 4g/mm

I'm unable to achieve FN even after several test.

Can anyone guide me how to achieve FN ?

Pravin
Singapore

Sent from my iPhone

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at
http://groups.google.com/group/materials-welding.
To view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/C06614E3-D0AA-42F0-9BA6-9A63A4690B7C%40gmail.com.
For more options, visit
https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/OF0E07B5AA.29750A0B-ONC2257E28.00286B21-C2257E28.00287CD9%40LocalDomain.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/4D12600C-500E-4EB0-B3B3-7C7083BD0379%40gmail.com.
For more options, visit https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...