Re: [MW:23176] How to qualify 1.5 mm thk to 60 mm thk in one wps

To qualify as per Sec IX,  for the above mentioned range you need to combine two PQR while making the WPS.

First PQR shall have T ( base metal thickness ) less than 10mm which will qualify the WPS from 1.5 mm to 2T.

Second PQR shall be made on say 30 mm Base metal thickness which will qualify the WPS from 5mm to 60 mm.

These two PQR can be combined while making a single  WPS provided all other essential variables are the same for both the PQR except for T.

If impact test requirements are there, then all the supplementary variables need to be considered.

Regards,

Anup

On 28 Apr 2015 13:03, "Jay Poojary" <jayogini@gmail.com> wrote:

Dear All,

To my knowledge,  it's not possible.  Thank you.

Jay Poojary,
QC Engineer
Signate Engineers & Consultancy

On Apr 28, 2015 10:57 AM, "joydev dalai" <joykolkata07@gmail.com> wrote:
It is not possible 

On Tue, Apr 28, 2015 at 10:39 AM, pradip kumar Sil <pradipsil@gmail.com> wrote:
asme sec ix

On Mon, Apr 27, 2015 at 9:12 AM, S.Mohammed <mohd52100@gmail.com> wrote:
as per which code?

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/31aa6d1b-9b75-459d-959a-c4d89cb70877%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAB%3DAs8kb4JmB9Y7NwbsaehrNjhHeTyS551%2BUDU_hUW1785kDXg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.



--



Best Regards,

Joydev Dalai
Sr. Engineer - QA/QC
Kalpataru Power Transmission Ltd
KJPL Project,(Spread-1)
Mob :- +91-7728885768

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFQz-VL80TEWrH%3D5HscjuPUd3ELOwa08Rqbf09%3Dwu_9JrjW2hg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAAcO%3DyRcmuP1a1L6A68Zqk3L%2B2qPycA2MF%2BbUvYd6y%3DbxTttXA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJsQutZjNXBnN_6jXBqXwj3LB6%2BO4qVOJ9Q5xdUC%2B7LF59DxZg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...