[MW:22332] Nap corrosion requirement and any tests to verify compliance of clad plates to Nap corrosion

Dear experts,

 

Request your kind help for below requirement.

 

There is partial clad vertical column i.e. bottom half vessel is clad SA 264(SA 516 Gr 70N+SA 240 TP 316L) and top half vessel is Plain carbon steel with corrosion allowance. Client said that bottom clad is due to Nap corrosion possibility of process liquid.

 

1.      Is there any possible test to prove compliance to Nap corrosion test requirement in case Mo content is 2.06 % (and not as high as 2.5%)?

2.      Is there any lining like epoxy, glass flake or any other lining which can be applied to avoid high Mo content requirements.

 

Please advise asap.

 

Regards



***DISCLAIMER NOTICE: ***
"The information contained in this email and/or any attachment hereto is strictly confidential and privileged. If you are not the intended recipient, and/or have received this email in error, you must not copy, disseminate or disclose the contents of this message and/or any attachment to any other person. Please notify the sender and delete this message and any attachment from your system. KNM accepts no liability in respect of prohibited and unauthorised use by an unintended addressee or recipient. Any personal views or opinions expressed by the sender shall be understood as neither given nor endorsed by KNM or any of the companies within the Group. Although this email and/or any attachment is believed to be free of any virus or other defect which may affect any computer system into which it is received and opened, it is the responsibility of the recipient to ensure that it is virus-free and KNM accepts no responsibility for any loss or damage arising in any way from the use thereof."

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...