Re: [SUSPECTED SPAM] Re: [MW:14236] Hardness value without PWHT

Dear friend
hardness can also be reduced by suitable electrode selection; (if proper electrode select that have low carbon content) then hardness can easy controllable but may reduce its strenght.
On Tue, May 8, 2012 at 8:04 AM, pgoswami <pgoswami@quickclic.net> wrote:
Pradip,

I do not think hardness control would be easy without any PWHT. It may be
advisable to talk to your client to have some form of PWHT  done in situ.
Either pad heating or flame heating.

Thanks.


Pradip Goswami,P.Eng.IWE
Welding & Metallurgical Specialist
Ontario, Canada.
Email-pgoswami@sympatico.ca,
[mailto:materials-welding@googlegroups.com] On Behalf Of pradip kumar sil
Sent: Friday, May 04, 2012 12:56 AM
To: materials-welding@googlegroups.com
Cc: pgoswami@quickclic.net
Subject: Re: [SUSPECTED SPAM] Re: [MW:14180] Hardness value without PWHT

Dear Sir,
 I did PQR as per your suggested WPS but hardness is coming still more i.e
230 to 287 BHN  in weld zone in P-4 material. Pls guide me how can i control
the hardness without PWHT .
Thanks in advance.
Regards
Pradip

On 4/20/12, pgoswami <pgoswami@quickclic.net> wrote:
> Pradip,
>
> See these guidelines (PQR) below. This would be useful.Hardness > 250
> HV is possible in P4 material, without PWHT.
>
> Let know.
>
> Thanks
>
>
> Pradip Goswami,P.Eng.IWE
> Welding & Metallurgical Specialist & Consultant Ontario, Canada.
> Email-pgoswami@sympatico.ca,
>  <mailto:pgoswami@quickclic.net> pgoswami@quickclic.net
>
>
>
>
>
>
>
> -----Original Message-----
> From: materials-welding@googlegroups.com [
> <mailto:materials-welding@googlegroups.com>
> mailto:materials-welding@googlegroups.com] On Behalf Of pradip kumar sil
> Sent: Wednesday, April 18, 2012 2:32 AM
> To: materials-welding@googlegroups.com
> Cc: pgoswami
> Subject: Re: [SUSPECTED SPAM] Re: [MW:14119] Hardness value without PWHT
>
> Dear Sir,
> These are reformer tubes to header  under B 31.3.
> As per design wall temperature are forecasted 200 to 220 degree
centigrade.
> Considering that the elastic range of of P-11 material in ASME 31.3 is
> defined upto 482 degree centigrade & creep range goes upto 649 degree
> centigrade. The operating temp can not taken as high.
> In our application  hydrogen partial pressure is 14 bar. ASME 31.3 allows
to
> weld 7.5 mm thickness without PWHT. If we increase preheat temperature we
> will get any benefit. Guide me how can i control hardness in these case.
> Regards
> Pradip
>
>
>
>
>
> On 4/14/12, james gerald <gerry_tup@yahoo.com> wrote:
>> 225BHN hardness specified is for Weldment which includes weld metal,
>> HAZ & BM. PWHT is one of the method of reducing hardness.
>>
>> Other methods are Controlled cooling t8/5 which can be achieved by
>> increasing the preheat. Preheat can be increased just below Mf
>> temperature and try the Hardness values.
>>
>> You could try with a temper bead welding technique. There are
>> different methods of temper bead welding technique and you can select
>> the suitable one for your case eg a half bead technioque.
>>
>> Thanks & Regards
>>
>>
>> J.Gerald Jayakumar
>> 0091-9344954677
>>
>>
>> ________________________________
>>  From: Ramchandra vichare <vicharerke@indiatimes.com>
>> To: materials-welding@googlegroups.com
>> Cc: pgoswami <pgoswami@quickclic.net>
>> Sent: Friday, April 13, 2012 2:43 PM
>> Subject: [SUSPECTED SPAM] Re: [MW:14106] Hardness value without PWHT
>>
>>
>> ----- Original Message -----
>>
>>
>> Dear friend,
>> First of all pl confirm which welding procedure you used
>> (i.e.GTAW+SMAW),or any one?
>>
>> See if you use welding technique GTAW by ER80SB2 + SMAW by E8018B2
>> hardness value will may be in controll.
>> Pl try & revert.
>>
>> Regards,
>> RK Vichare
>>
>>
>> From: pradip kumar sil <pradipsil@gmail.com>
>> To: materials-welding@googlegroups.com
>> Cc: pgoswami <pgoswami@quickclic.net>
>> Sent: Thu, 12 Apr 2012 10:50:16 +0530 (IST)
>> Subject: [MW:14104] Hardness value without PWHT
>>
>> Dear experts,
>> I have faced regarding hardness issue on ASTM A 335 GR P-11 material.
>> Pipe thickness is 7.5mm.  Without PWHT hardness is coming around 275
>> to 289 BHN  on weld zone & 250 260 BHN on HAZ zone & parent material
>> hardness is 197 to 204 BHN. Due to inside refractory material PWHT is
>> not possible.
>> My question is as per ASME B-31.3/ ASME SEC II PART A hardness value
>> of this material is 225 BHN ( MAX).  There is any specification for
>> weld zone / HAZ zone hardness value.
>> Can anybody give an idea to reduce the hardness without PWHT  if it is
>> not acceptable limit.
>> Thanx in advance.
>>
>> Regards
>> Pradip
>>
>> --
>> To post to this group, send email to
>> materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>>  <http://materials-welding.blogspot.com/>
> http://materials-welding.blogspot.com/
>> The views expressed/exchnaged in this group are members personel views
>> and meant for educational purposes only, Users must take their own
>> decisions w.r.t. applicable code/standard/contract documents.
>>
>> --
>> To post to this group, send email to
>> materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>>  <http://materials-welding.blogspot.com/>
> http://materials-welding.blogspot.com/
>> The views expressed/exchnaged in this group are members personel views
>> and meant for educational purposes only, Users must take their own
>> decisions w.r.t. applicable code/standard/contract documents.
>>
>> --
>> To post to this group, send email to
>> materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>>  <http://materials-welding.blogspot.com/>
> http://materials-welding.blogspot.com/
>> The views expressed/exchnaged in this group are members personel views
>> and meant for educational purposes only, Users must take their own
>> decisions w.r.t. applicable code/standard/contract documents.
>>
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> <http://materials-welding.blogspot.com/>
> http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>
>
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and
meant for educational purposes only, Users must take their own decisions
w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.