[MW:13248] RE: 13243] IMPACT TEST -SUB SIZE

Dear Elumalai,

Nice to hear from you.

 

If we do impact testing at the specimen size of 10 X 7.2mm (i.e 80% of 9mm) there is no need of reduction in temperature

 

If we are using a sub size of 5mm (i.e lesser than 80% of original) then we have to go for reduction in temperature

As per AWS D1.1- 2008 table 4.14 note (C ) and table 4.15 for this case further reduction of 11.1°C is required  i.e -29 – 11 = -41.1°C (9mm-5mm)

 

The observed energy required for sub size as per note of table 4.15 and ASTM A370 Table 9 is 14 Joules average and 11 joules individual

 

 

 

 

 

 

 

 

 

 

 

Cheers

MM

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Sundaram Elumalai
Sent: Wednesday, December 21, 2011 8:16 AM
To: materials-welding@googlegroups.com
Subject: [MW:13243] IMPACT TEST -SUB SIZE

 

Hi,

 

Now we are qualifying two new PQR for new project for less base metal

thick. (9mm). Code AWS D1.1

 

ROOT / HOT Pass              -GTAW (deposited 4mm)

Fill/Cap                                - SMAW (deposited 5mm)

 

We need to perform the impact test as per Client Welding spec for each process.

In this case, we have to go for Sub size with temperature reduction.

 

Client Welding spec requirement is minimum - 29 °C. 

 

If I go with 10x5mm sub size, I need to reduce 11.1 °C  and test to be

done at -40.1°C. (  -29 -11.1) 

Then Joule value will considered as per ASTM 370,16 J from the below

second table.

 

Is it correct ?

 

With Kind Regards,

 

S.Elumalai.

******************************************************************************************
CONFIDENTIALITY NOTICE
This e-mail and any attachment are confidential and may be privileged or otherwise protected from disclosure. It is solely intended for the person(s) named above. If you are not the intended recipient, any reading, use, disclosure, copying or distribution of all or parts of this e-mail or associated attachments is strictly prohibited. If you are not an intended recipient, please notify the sender immediately by replying to this message or by telephone and delete this e-mail and any attachments permanently from your system.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...