RE: [MW:4125] Low hydrogen electrodes for station piping

Low hydrogen electrodes are indeed less susceptible to HIC and tend to give better low temperature impact values. There are as you probably know good suppliers of low hydrogen vertical down electrodes for pipeline welding.

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of John Du Plessis
Sent: 21 January 2010 09:03
To: materials-welding@googlegroups.com
Subject: RE: [MW:4119] Low hydrogen electrodes for station piping

 

 

 

I disagree. Low hydrogen is not stronger weld metal than cellulosic – check the AWS strength classes. Do however agree that low hydrogen weld metal is less susceptable to hydrogen induced cracking

 

John du Plessis

Technology Manager

 

Tel: +27 (11) 298 2100

Tel: +27 (11) 298 2103 (Direct)

Fax: +27 (11) 836 6014

Mobile:+27  (11) 82 883 4970

www.saiw.co.za

 

This email and any files transmitted with it are confidential and may be legally privileged. They are intended solely for the use of the individual or entity to whom they are addressed. Access to this e-mail by anyone else is unauthorised, and any disclosure, copying, distribution or other use of this e-mail is prohibited and may be unlawful. We will not under any circumstances have any responsibility or liability arising out of or in connection with any unauthorised use of this e-mail. If you have received this email in error please notify the sender before deleting it.


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of michael lawrence
Sent: 21 January 2010 12:51 AM
To: materials-welding@googlegroups.com
Cc: michael lawrence
Subject: Re: [MW:4114] Low hydrogen electrodes for station piping

 

because low hydrogen is a stronger weld material and less hydrogen content so less cracking in the weld and heat afected zone area.

 

 

regards

mike.

----- Original Message -----

From: Gulam kader

Sent: Wednesday, January 20, 2010 9:54 AM

Subject: [MW:4104] Low hydrogen electrodes for station piping

 

Dear all,

 

why we are always using low hydrogen electrodes for station piping instead of cellulose electrode. somebody can explain please?

 

Regards,

 

Gulam Kader


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



No virus found in this incoming message.
Checked by AVG - www.avg.com
Version: 8.5.432 / Virus Database: 270.14.151/2633 - Release Date: 01/19/10 17:49:00

 


This email message and accompanying data are for the sole use of the intended recipient(s) and may contain confidential information and/or copyright material. Unauthorised use, copying or disclosure of any of it is prohibited and may be unlawful. If you received this email message in error, please notify us immediately and erase all copies of this message and attachments. Global Energy scans and monitors incoming and outgoing mail in accordance with its IT Policy - this email has been scanned for viruses. Global Energy Holdings Ltd and its subsidiaries accept no liability for direct, indirect or consequential damages arising from the alteration of the contents of this message by a third party, or as a result of a virus being passed on.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...