Skip to main content

[MW:1173] Re: 1150] SAW - For Single sided joint

IF code and specification permit try Cellulose Electrode for root and
followed by SAW.

I feel single bevel 45 degree V s not recommended groove for SAW. End
result of such groove may endup in having side wall lack of fusion.

Suggest to go ahead with J type groove atleast.

Regards

Paresh


On 9/22/08, Bathula Raghuram (Mumbai - PIPING) <R.Bathula@ticb.com> wrote:
> Why not GTAW+SAW? Full SAW may not give you full penetration + defect free
> in UT
>
> -----Original Message-----
> From: materials-welding@googlegroups.com
> [mailto:materials-welding@googlegroups.com]On Behalf Of PREM SHANKARDUTT
> NAUTIYAL
> Sent: Saturday, September 20, 2008 4:36 PM
> To: materials-welding@googlegroups.com
> Subject: [MW:1150] SAW - For Single sided joint
>
>
>
>
> Dear Friends
>
> We are trying to establish SAW for single sided joint. The base metal is
> SA516Gr.70. The joint is 25mm thick. The joint is a single bevel groove but
> joint with included angle of 45degree ( one member is vertical and there is
> bevel on other member).The final NDT is UT.
> Presently we are welding this joint with TIG+SMAW.The joint is circular
> hence ideal for SAW.
> Now we want to try to weld this single sided joint completely with SAW. This
> is for productivity improvement.
> Is it possible to weld this joint having no access from other side with SAW
> completely ?
> Can we keep zero gap, zero rootface, and achieve full penetration joint with
> SAW??
> If yes what should be the parameters, wire dia., etc.
> We dont want to use any ceramic backing.
> Can anyone suggest how to weld this joint completely with SAW.
> This is a development activity. Please share your experience...
>
> Regards
>
> Prem Nautiyal
>
>
> PREM S NAUTIYAL
> CELL : 9820313278
>
>
> <http://adworks.rediff.com/cgi-bin/AdWorks/click.cgi/www.rediff.com/signature-home.htm/1050715198@Middle5/2401775_2394076/2397136/1?PARTNER=3&OAS_QUERY=null>
> Ebay
>
>
>
>
>
> >
>

--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...