Skip to main content

[MW:1163] Re: SAW filler wire parameters

 
We have used 650A,34V,450mm/min Travel speed.
Result: slag removal little difficult, interbead LOF..

Please advise experts the correct welding parameters ???

On Mon, 22 Sep 2008 Muhammed Ibrahim wrote :
>450-550 Amp, 30-32 V, 50cm per minute travel speed.
>
>
>
>
>2008/9/19 PREM SHANKARDUTT NAUTIYAL <prem_nautiyal@rediffmail.com>
>
> >
> > Dear Friends
> >
> > We are presently trying to use a local make 4.8mm dia SAW filler wire
> > (EM12K)in place of 3.15mm dia.
> > Can anyone tell us the correct welding parameters like:
> > current, voltage, travel speed,etc for 4.8mm dia wire..
> > The base metal is SA516Gr.70, the thickness is 70mm. The joint is single
> > bevel groove joint with no access from other side. Presently we weld first 2
> > passes with TIG, Then 2 passes of SMAW and then subsequent passes with
> > SAW-3.15mm dia. Now we want to use 5.0mm dia SAW wire. So what should be the
> > welding parameters ? We have tried various parameters for SAW(4.8mm dia
> > wire) but failed to get good weld finish /UT. We have a 1200A Lincoln Power
> > source.
> > The joint calls for UT.
> >
> > Regards
> >
> > Prem Nautiyal
> > PREM S NAUTIYAL
> > CELL : 9820313278
> >
> >  [image: Ebay]<http://adworks.rediff.com/cgi-bin/AdWorks/click.cgi/www.rediff.com/signature-home.htm/1050715198@Middle5/2401775_2394076/2397136/1?PARTNER=3&OAS_QUERY=null>
> > >
> >
>
>
>--
>Thanks & Regards
>Muhammed Ibrahim PK
>
>>

PREM S NAUTIYAL
CELL : 9820313278

--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...
Ebay