Skip to main content

Re: [MW:35579] Advice for FCAW qualification

Dear Sir,



I am grateful to you for supporting me, but if you have any welding matrix then please send it, I will get the reference




Thanks & Regards
Mr. NITESH
Mob No. : 9939998302

On Sun, Apr 27, 2025 at 3:10 PM Nambirajan Avudaiappan <nambirajanavudaiappan@gmail.com> wrote:
Weld Pass Process Filler Filler Metal Dia. Current Volts Current Type & Polarity Travel Speed (mm/min) Heat Input
Layers No. Metal (A) (A) KJ/mm
1 1 FCAW E71T-1C Ø 1.2 120-160 18-25 DCEP 175 0.74
2 2 FCAW E71T-1C Ø 1.2  150-180 20-25 DCEP 300 0.64
3 3 FCAW E71T-1C Ø 1.2  150-180 20-25 DCEP 300 0.64
4 4 FCAW E71T-1C Ø 1.2  150-180 20-25 DCEP 300 0.64

Interpass cleaning :- Grinding and brushing.

Weld position 1 g only .

Appreciate your feedback Mr.Sridhar


On Sun, 27 Apr 2025 at 11:21, sridhar cn <sridharcn305@gmail.com> wrote:
You have not spelled out the weld parameters like,
Current, Voltage, Stick out, Travel speed, and interpass cleaning, power source weld position etc.
CS.

On Sun, 27 Apr 2025 at 12:00, Nambirajan Avudaiappan <nambirajanavudaiappan@gmail.com> wrote:

Hi shridar,

Thank you for your advice.

I am currently using Hyundai brand (E71T-1C) 1.2 mm filler wire.


On Sat, 26 Apr 2025 at 18:44, sridhar cn <sridharcn305@gmail.com> wrote:
Dear Mr. Nambirajan,
The reasons for slag inclusion could be due to 
* high welding travel speed,
* improper in between pass cleaning,
* weld parameters like low current, low/high voltage, improper torch angle,
* align the weld beads properly to avoid slag entrapment in between,
* use 15 deg. drag angle during welding,
* use a power brush instead of a hand brush to clean the slag between each pass etc.
* also check your filler wire. Use a basic wire instead of rutile filled FCAW wire.
* avoid  a low cost Chinese made power source (if it is in use currently) and go for a 
   branded one like Lincoln, Esab, OTC (Japan make) etc.
Please provide the welding parameters you are using presently for your 1.2 mm size filler wire If it is OK
rgds,
C Sridhar.
-----------------------------------------------------------------------------------------------------------------------------



On Sat, 26 Apr 2025 at 18:37, Nambirajan Avudaiappan <nambirajanavudaiappan@gmail.com> wrote:

Dear Experts,

We are currently conducting FCAW qualification on a 25mm thick SA-36 material plate. However, we are facing issues with slag inclusion during the process.

Despite performing thorough cleaning after every pass, slag inclusions are still observed.
We kindly request your advice and recommendations on how we can take effective control measures to eliminate this problem.

Your expert guidance would be highly appreciated.

Thank you and best regards,

Nambirajan A

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJuyB2Xo-oR1On%3D5v6oiUvEPu-%2BG%2Bbzo%2Bf1DMR_3PXWXiEacuA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYigbvZdNuXzQH_n5Kxho0OZDNYsiM0kB9fPNgAwEx_0KAg%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJuyB2WvPyb0fmArUMC8VopDmqaMaOPS157JwOeGMj_%2BsdaPtg%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYiiDNm6NhAmMXzcgWPOad4wt4Zcx%2Bcx5h44HnJdTh6a0Zg%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJuyB2V%3DdB_QKyMW_fziznj%2B86piSY8vZu9Q%2BhaFr7rusYjoPQ%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CALE9gmm1B%3DCn_aqpTntCd0tRSp5iZVNED616Frfxr0VnbBmiVg%40mail.gmail.com.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...